Materion Performance Alloys’ Alloy 390E is a copper beryllium alloy that provides a unique combination of high strength, high electrical conductivity, and excellent formability. Copper beryllium alloys are well known for their superior stress relaxation resistance and fatigue strength. This blend of properties provides engineers the flexibility to design small form factor signal and power interconnects that can be used in harsh environments.

Related Standards

This material data has been provided by Materion Brush GmbH.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

23.0 °C

8.83 g/cm³

Show Supplier Material materials with Density of 8.83 g/cm³

Dimension

PropertyValueComment

Thickness

0.05 - 0.38 mm

Show Supplier Material materials with Thickness of 0.05 - 0.38 mm

thinner gauges maybe available upon request

Width

1.27 - 406.5 mm

Show Supplier Material materials with Width of 1.27 - 406.5 mm

Mechanical

PropertyTemperatureValueComment

Bendability 90°, bw

23.0 °C

1 - 3.5 [-]

Show Supplier Material materials with Bendability 90°, bw of 1 - 3.5 [-]

depending on the thickness

Bendability 90°, gw

23.0 °C

1 - 3.5 [-]

Show Supplier Material materials with Bendability 90°, gw of 1 - 3.5 [-]

depending on the thickness

Elastic modulus

23.0 °C

138 GPa

Show Supplier Material materials with Elastic modulus of 138 GPa

Elongation

23.0 °C

2 %

Show Supplier Material materials with Elongation of 2 %

for strip thicker than 0.10 mm

Fatigue strength

23.0 °C

552 MPa

Show Supplier Material materials with Fatigue strength of 552 MPa

10⁷ cycles, R=0

Hardness, Vickers

23.0 °C

300 [-]

Show Supplier Material materials with Hardness, Vickers of 300 [-]

Tensile strength

23.0 °C

986 MPa

Show Supplier Material materials with Tensile strength of 986 MPa

Yield strength Rp0.2

23.0 °C

951 MPa

Show Supplier Material materials with Yield strength Rp0.2 of 951 MPa

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

23.0 °C

1.76E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.76E-5 1/K

Specific heat capacity

23.0 °C

419 J/(kg·K)

Show Supplier Material materials with Specific heat capacity of 419 J/(kg·K)

Thermal conductivity

23.0 °C

208 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 208 W/(m·K)

Electrical

PropertyValue

Specific Electrical conductivity

42 % IACS

Show Supplier Material materials with Specific Electrical conductivity of 42 % IACS

Technological properties

Property
Application areas