Alloy 25 Tube TB00 (C17200)

Alternative and trade names
Alloy 25 (C17200) Tube
Want to keep this datasheet? Save it now in your required format

Description

Alloy 25 Tube from Materion Performance Alloys provides the highest strength of any copper alloy, with electrical conductivity considerably greater than other high strength copper alloys. This alloy features high fatigue strength and magnetic permeability approaching unity.

Related Standards

This material data has been provided by Materion Brush GmbH.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

23.0 °C

8.36 g/cm³

Show Supplier Material materials with Density of 8.36 g/cm³

Dimension

PropertyValue

Outside diameter

19.1 - 406 mm

Show Supplier Material materials with Outside diameter of 19.1 - 406 mm

Wall thickness

10-20% of outside diameter

Mechanical

PropertyTemperatureValue

Elastic modulus

23.0 °C

131 GPa

Show Supplier Material materials with Elastic modulus of 131 GPa

Elongation

23.0 °C

20 - 75 %

Show Supplier Material materials with Elongation of 20 - 75 %

Tensile strength

23.0 °C

410 - 590 MPa

Show Supplier Material materials with Tensile strength of 410 - 590 MPa

Yield strength Rp0.2

23.0 °C

130 - 250 MPa

Show Supplier Material materials with Yield strength Rp0.2 of 130 - 250 MPa

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

23.0 °C

1.75E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.75E-5 1/K

Melting point

870 °C

Show Supplier Material materials with Melting point of 870 °C

Thermal conductivity

23.0 °C

105 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 105 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

23.0 °C

5.8E-6 - 6.9E-6 Ω·m

Show Supplier Material materials with Electrical resistivity of 5.8E-6 - 6.9E-6 Ω·m

Specific Electrical conductivity

25 - 30 % IACS

Show Supplier Material materials with Specific Electrical conductivity of 25 - 30 % IACS

Magnetic

PropertyTemperatureValueComment

Relative magnetic permeability

23.0 °C

1 [-]

Show Supplier Material materials with Relative magnetic permeability of 1 [-]

max.

Chemical properties

PropertyValueComment

Beryllium

1.8 - 2 %

Show Supplier Material materials with Beryllium of 1.8 - 2 %

Cobalt

0.2 %

Show Supplier Material materials with Cobalt of 0.2 %

min. Nickel + Cobalt

Copper

Balance

Iron

0.6 %

Show Supplier Material materials with Iron of 0.6 %

max., Nickel + Cobalt + Iron

Lead

0.2 - 0.6 %

Show Supplier Material materials with Lead of 0.2 - 0.6 %

Nickel

0.2 %

Show Supplier Material materials with Nickel of 0.2 %

min. Nickel + Cobalt

Technological properties

Property
Application areas

Typical applications include bushings and bearings for aircraft as well as drill collars and instrument housings for oil and gas exploration.