Alloy 174 (C17410) TH04 Strip

Want to keep this datasheet? Save it now in your required format

Description

Materion Performance Alloys’ Alloy 174 strip is a mill hardened copper beryllium strip alloy designed for use in the Automotive, Appliance, and DataCom/TeleCom markets. It provides high yield and fatigue strength with high electrical conductivity and good resistance to stress relaxation. Typical applications include high reliability automotive terminals and spring contacts for switches and relays.

Related Standards

This material data has been provided by Materion Brush GmbH.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

23.0 °C

8.8 g/cm³

Show Supplier Material materials with Density of 8.8 g/cm³

Dimension

PropertyValue

Thickness

0.05 - 2 mm

Show Supplier Material materials with Thickness of 0.05 - 2 mm

Width

1.27 - 406.5 mm

Show Supplier Material materials with Width of 1.27 - 406.5 mm

Mechanical

PropertyTemperatureValueComment

Bendability 90°, bw

23.0 °C

5 [-]

Show Supplier Material materials with Bendability 90°, bw of 5 [-]

for strip with 0.25mm and thinner.

Bendability 90°, gw

23.0 °C

1.2 [-]

Show Supplier Material materials with Bendability 90°, gw of 1.2 [-]

for strip with 0.25mm and thinner.

Elastic modulus

23.0 °C

138 GPa

Show Supplier Material materials with Elastic modulus of 138 GPa

Elongation

23.0 °C

7 - 17 %

Show Supplier Material materials with Elongation of 7 - 17 %

Fatigue strength

23.0 °C

585 - 655 MPa

Show Supplier Material materials with Fatigue strength of 585 - 655 MPa

10⁸ cycles R=0 (Unidirectional)

Hardness, Vickers

23.0 °C

210 - 278 [-]

Show Supplier Material materials with Hardness, Vickers of 210 - 278 [-]

Tensile strength

23.0 °C

760 - 895 MPa

Show Supplier Material materials with Tensile strength of 760 - 895 MPa

Yield strength Rp0.2

23.0 °C

690 - 830 MPa

Show Supplier Material materials with Yield strength Rp0.2 of 690 - 830 MPa

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

23.0 °C

1.76E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.76E-5 1/K

Melting point

1020 °C

Show Supplier Material materials with Melting point of 1020 °C

Thermal conductivity

23.0 °C

230 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 230 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

23.0 °C

2.9E-6 - 3.8E-6 Ω·m

Show Supplier Material materials with Electrical resistivity of 2.9E-6 - 3.8E-6 Ω·m

Specific Electrical conductivity

45 - 60 % IACS

Show Supplier Material materials with Specific Electrical conductivity of 45 - 60 % IACS

Chemical properties

PropertyValue

Beryllium

0.15 - 0.5 %

Show Supplier Material materials with Beryllium of 0.15 - 0.5 %

Cobalt

0.35 - 0.6 %

Show Supplier Material materials with Cobalt of 0.35 - 0.6 %

Copper

Balance

Technological properties

Property
Application areas

Typical applications include high reliability automotive terminals and spring contacts for switches and relays.