Structural Epoxy Resin T26 (EP-UD tape)

Want to keep this datasheet? Save it now in your required format

Description

Т26 is a single part low viscosity epoxy infusion resin, coated with UD tape, developed for high-loaded structures. T26 offers simple and flexible processing due to low viscosity at relatively low impregnation temperatures (110°С). T26 was developed specially for RTM and vacuum infusion molding, to produce laminates with low porosity and extremely high mechanical performance, especially in crack resistance. It shows the following features and properties:


  • One-part resin designed specifically for high-temperature infusion or RTM
  • Wide processing window > 7 hours at 110°C
  • Curing at 180°C provides glass transition temperature of 205°C
  • High wet glass transition temperature —172°C
  • Very high resistance to impact
  • Operating temperatures from –60°C to 150°C
  • This material data has been provided by Matmatch.

    "Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
    All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
    Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

    Ashby charts

    Properties

    Mechanical

    PropertyTemperatureValueComment

    Compressive strength

    25.0 °C

    1210 MPa

    Show Material materials with Compressive strength of 1210 MPa

    ASTM D6641

    80.0 °C

    920 MPa

    Show Material materials with Compressive strength of 920 MPa

    ASTM D6641

    120.0 °C

    772 MPa

    Show Material materials with Compressive strength of 772 MPa

    ASTM D6641

    150.0 °C

    691 MPa

    Show Material materials with Compressive strength of 691 MPa

    ASTM D6641

    Compressive strength, transverse

    23.0 °C

    166 MPa

    Show Material materials with Compressive strength, transverse of 166 MPa

    ASTM D6641

    Elastic modulus

    23.0 °C

    108 GPa

    Show Material materials with Elastic modulus of 108 GPa

    ASTM D3039

    Elastic modulus, transverse

    23.0 °C

    7 GPa

    Show Material materials with Elastic modulus, transverse of 7 GPa

    ASTM D3039

    Shear modulus, G₁₂

    23.0 °C

    4 GPa

    Show Material materials with Shear modulus, G₁₂ of 4 GPa

    ASTM D5379

    Shear strength, τ₁₂

    23.0 °C

    80 MPa

    Show Material materials with Shear strength, τ₁₂ of 80 MPa

    Shear strength, τ₁₃

    25.0 °C

    69 MPa

    Show Material materials with Shear strength, τ₁₃ of 69 MPa

    ASTM D2344

    80.0 °C

    46 MPa

    Show Material materials with Shear strength, τ₁₃ of 46 MPa

    ASTM D2344

    120.0 °C

    34 MPa

    Show Material materials with Shear strength, τ₁₃ of 34 MPa

    ASTM D2344

    150.0 °C

    28 MPa

    Show Material materials with Shear strength, τ₁₃ of 28 MPa

    ASTM D2344

    Unlock all property charts

    Tensile strength

    23.0 °C

    1886 MPa

    Show Material materials with Tensile strength of 1886 MPa

    ASTM D3039

    Tensile strength, transverse

    23.0 °C

    59 MPa

    Show Material materials with Tensile strength, transverse of 59 MPa

    ASTM D3039

    Technological properties

    Property
    Application areas

    Drones;Sports equipment: Frame, wheels, seat, seat post, handlebar, head stem and crank arm of a sports bicycle are made of carbon composite;Geometry strengthen elements: Experimental stringer panel

    Processing history

    Samples for testing were obtained by vacuum infusion based on T26 resin and UD tape covered by veil 11424 (200 g/m2, 12K, 4.5 GPa/240 GPa).

    Processing methods

    Preheat the resin to 60-90°С in its container for transfer to the resin pot. Degas the resin for 30-40 minutes while heating to 90°С. Preheat the tool to 100-110°С (or to 115-120°С for parts having complex shape or for UD parts). Maintaining resin pot temperature of 95 °С and tool temperature of 100-115 °С, begin resin infusion. After complete impregnation increase tool temperature at 2°С/min to 180°С. Dwell at 180°С for 3 h. Cool the tool to 90°С at <5°С/min before releasing part from tool.