ОоА prepreg B180 CF08 [0,+45, -45,90]nS

Want to keep this datasheet? Save it now in your required format

Description

В180 is a prepreg based on epoxy carbon fiber reinforced resin for producing details with operating temperatures up to 150°C. Out-of-autoclave prepreg technology has the most advantages of autoclave. The autoclave is not required for processing the prepreg B180. Curing takes place in a vacuum bag, with the technology of the package laminating slightly different from the vacuum infusion. It shows the following features and properties:


  • High mechanical performance
  • Possibility of application in loaded parts at service temperatures up to 120°C
  • Less stringent requirements for working staff
  • Glass transition temperature 154°C
  • Out of autoclave processing
  • This material data has been provided by Matmatch.

    "Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
    All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
    Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

    Ashby charts

    Properties

    Mechanical

    PropertyTemperatureValueComment

    Compressive modulus

    23.0 °C

    71 MPa

    Show Material materials with Compressive modulus of 71 MPa

    ASTM D695, Lamina

    Compressive modulus laminate

    25.0 °C

    48 GPa

    Show Material materials with Compressive modulus laminate of 48 GPa

    85.0 °C

    47 GPa

    Show Material materials with Compressive modulus laminate of 47 GPa

    Compressive strength

    23.0 °C

    802 MPa

    Show Material materials with Compressive strength of 802 MPa

    ASTM D6641, Lamina

    Compressive strength laminate

    85.0 °C

    594 MPa

    Show Material materials with Compressive strength laminate of 594 MPa

    85% wet

    Elastic Modulus laminate

    25.0 °C

    50 GPa

    Show Material materials with Elastic Modulus laminate of 50 GPa

    85.0 °C

    46 GPa

    Show Material materials with Elastic Modulus laminate of 46 GPa

    120.0 °C

    46 GPa

    Show Material materials with Elastic Modulus laminate of 46 GPa

    Unlock all property charts

    Elastic modulus

    23.0 °C

    60 GPa

    Show Material materials with Elastic modulus of 60 GPa

    ASTM D3039, Lamina

    Shear modulus, G₁₂

    23.0 °C

    5.7 GPa

    Show Material materials with Shear modulus, G₁₂ of 5.7 GPa

    ASTM D5379, Lamina

    Shear strength, τ₁₂

    23.0 °C

    126 MPa

    Show Material materials with Shear strength, τ₁₂ of 126 MPa

    Shear strength, τ₁₃

    23.0 °C

    79 MPa

    Show Material materials with Shear strength, τ₁₃ of 79 MPa

    ASTM D2344, Lamina

    Tensile strength

    23.0 °C

    871 MPa

    Show Material materials with Tensile strength of 871 MPa

    ASTM D3039, Lamina

    Tensile strength laminate

    85.0 °C

    636 MPa

    Show Material materials with Tensile strength laminate of 636 MPa

    85% wet

    Technological properties

    Property
    Application areas

    Marine: The shells of boats and sport catamarans can be made of composites;Car tuning: The composite material provides solutions for automotive parts to be light-weighted, stylish and aesthetic;Sports equipment: Frame, wheels, seat, seat post, handlebar, head stem and crank arm of a sports bicycle are made of carbon composite

    Processing history

    Reinforcing filler: carbon fabric 22508 (twill 2x2, 200 g/m2, HTA40). Carbon plastic is produced by vacuum molding.

    Processing methods

    Holding at a temperature of 25-30°C, for 12 hours, a vacuum of -1 bar. Heating 2°C/min. up to 120°C, holding at 120°C for 180 minutes. Heating 2°C/min. up to 180°C, holding at 180°C for 180 minutes, cooling no faster than 5°C/min. up to 50°С.