General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 8.9 - 8.94 g/cm³ Show Material materials with Density of 8.9 - 8.94 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 95 - 98 GPa Show Material materials with Elastic modulus of 95 - 98 GPa | Typical for Wrought Copper Pure / Low Alloyed Copper |
Elongation | 20.0 °C | 5 % Show Material materials with Elongation of 5 % | |
Elongation A10 | 20.0 °C | 4 % Show Material materials with Elongation A10 of 4 % | |
Elongation A100 | 20.0 °C | 3 % Show Material materials with Elongation A100 of 3 % | |
Poisson's ratio | 23.0 °C | 0.34 [-] Show Material materials with Poisson's ratio of 0.34 [-] | Typical for Wrought Copper Pure / Low Alloyed Copper |
Shear modulus | 23.0 °C | 48 GPa Show Material materials with Shear modulus of 48 GPa | Typical for Wrought Copper Pure / Low Alloyed Copper |
Tensile strength | 20.0 °C | 350 MPa Show Material materials with Tensile strength of 350 MPa | |
Yield strength Rp0.2 | 20.0 °C | 320 - 330 MPa Show Material materials with Yield strength Rp0.2 of 320 - 330 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 100.0 °C | 1.68E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.68E-5 1/K | |
200.0 °C | 1.73E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.73E-5 1/K | ||
300.0 °C | 1.77E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.77E-5 1/K | ||
Melting point | 965 - 1100 °C Show Material materials with Melting point of 965 - 1100 °C | Typical for Wrought Copper Pure / Low Alloyed Copper | |
Specific heat capacity | -150.0 °C | 282 J/(kg·K) Show Material materials with Specific heat capacity of 282 J/(kg·K) | |
-50.0 °C | 361 J/(kg·K) Show Material materials with Specific heat capacity of 361 J/(kg·K) | ||
20.0 °C | 386 J/(kg·K) Show Material materials with Specific heat capacity of 386 J/(kg·K) | ||
100.0 °C | 393 J/(kg·K) Show Material materials with Specific heat capacity of 393 J/(kg·K) | ||
200.0 °C | 403 J/(kg·K) Show Material materials with Specific heat capacity of 403 J/(kg·K) | ||
300.0 °C | 415 J/(kg·K) Show Material materials with Specific heat capacity of 415 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 305 W/(m·K) Show Material materials with Thermal conductivity of 305 W/(m·K) | |
50.0 °C | 310 W/(m·K) Show Material materials with Thermal conductivity of 310 W/(m·K) | ||
100.0 °C | 318 W/(m·K) Show Material materials with Thermal conductivity of 318 W/(m·K) | ||
200.0 °C | 326 W/(m·K) Show Material materials with Thermal conductivity of 326 W/(m·K) | ||
300.0 °C | 334 W/(m·K) Show Material materials with Thermal conductivity of 334 W/(m·K) | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical conductivity | 20.0 °C | 4.30E+7 S/m Show Material materials with Electrical conductivity of 4.30E+7 S/m |
50.0 °C | 4.10E+7 S/m Show Material materials with Electrical conductivity of 4.10E+7 S/m | |
100.0 °C | 3.70E+7 S/m Show Material materials with Electrical conductivity of 3.70E+7 S/m | |
200.0 °C | 3.40E+7 S/m Show Material materials with Electrical conductivity of 3.40E+7 S/m | |
300.0 °C | 3.00E+7 S/m Show Material materials with Electrical conductivity of 3.00E+7 S/m | |
Electrical resistivity | 20.0 °C | 2.2E-8 Ω·m Show Material materials with Electrical resistivity of 2.2E-8 Ω·m |
50.0 °C | 2.4E-8 Ω·m Show Material materials with Electrical resistivity of 2.4E-8 Ω·m | |
100.0 °C | 2.7E-8 Ω·m Show Material materials with Electrical resistivity of 2.7E-8 Ω·m | |
200.0 °C | 2.9E-8 Ω·m Show Material materials with Electrical resistivity of 2.9E-8 Ω·m | |
300.0 °C | 3.3E-8 Ω·m Show Material materials with Electrical resistivity of 3.3E-8 Ω·m | |
Chemical properties
Property | Value |
---|---|
Copper | 99.9 % Show Material materials with Copper of 99.9 % |
Phosphorus | 0.02 - 0.04 % Show Material materials with Phosphorus of 0.02 - 0.04 % |