EN 12163 Grade CuSn6 R550

Want to keep this datasheet? Save it now in your required format

Description

CuSn6, mat. No. CW425K, is comparable to the DIN-make CuSn6, mat. No. 2.1020, acc. to DIN 17662 : 1983-12. Properties of the CuSn-alloy are predominantly determined by the tin-content. Tensile strength, yield point and hardness increase according to the rising cold forming grade, elongation after fracture decreases. Electrical and thermal conductivity are lower than for pure copper. Very high resistance to corrosion, particularly to atmospheric influences, seawater, sulfite liquor, carbonated and salted mine water. The alloys are stress corrosion-proof. Processing properties: warm forming: medium cold forming: very good machinability: medium hard soldering: good soft soldering: good gas shielded welding: good burnishing: good Appliction: For all types of springs, especially in electrical industry, for connectors, hose and spring tubes, fabric and screening wires, gong bars. Further application in paper, cellulose and chemical industry, in shipbuilding and machine engineering. For the electrolytically tinned strip the coatings (Sn bright, Sn matt, Sn fuzed, SnPb) are listed by the application (better solderability, better corrosion resistance, reduction of the electrical contact resistance, better appearance) in the DIN EN 14436 : 2004-11 (Table 5)

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8.8 - 8.82 g/cm³

Show Material materials with Density of 8.8 - 8.82 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

110 - 130 GPa

Show Material materials with Elastic modulus of 110 - 130 GPa

Typical for Leaded Phosphor Bronze

Elongation A10

20.0 °C

5 %

Show Material materials with Elongation A10 of 5 %

Elongation A100

20.0 °C

4 %

Show Material materials with Elongation A100 of 4 %

Poisson's ratio

23.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Leaded Phosphor Bronze

Tensile strength

20.0 °C

550 MPa

Show Material materials with Tensile strength of 550 MPa

Yield strength Rp0.2

20.0 °C

500 MPa

Show Material materials with Yield strength Rp0.2 of 500 MPa

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

100.0 °C

1.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 1/K

200.0 °C

1.85E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.85E-5 1/K

650.0 °C

2.22E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.22E-5 1/K

800.0 °C

2.18E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2.18E-5 1/K

Max service temperature, long

0 - 150 °C

Show Material materials with Max service temperature, long of 0 - 150 °C

Specific heat capacity

20.0 °C

377 J/(kg·K)

Show Material materials with Specific heat capacity of 377 J/(kg·K)

Thermal conductivity

20.0 °C

75 W/(m·K)

Show Material materials with Thermal conductivity of 75 W/(m·K)

200.0 °C

98 W/(m·K)

Show Material materials with Thermal conductivity of 98 W/(m·K)

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical conductivity

20.0 °C

9.00E+6 S/m

Show Material materials with Electrical conductivity of 9.00E+6 S/m

200.0 °C

7.80E+6 S/m

Show Material materials with Electrical conductivity of 7.80E+6 S/m

Unlock all property charts

Electrical resistivity

20.0 °C

1.11E-7 Ω·m

Show Material materials with Electrical resistivity of 1.11E-7 Ω·m

200.0 °C

1.28E-7 Ω·m

Show Material materials with Electrical resistivity of 1.28E-7 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Iron

0.1 %

Show Material materials with Iron of 0.1 %

Lead

0.02 %

Show Material materials with Lead of 0.02 %

Nickel

0.2 %

Show Material materials with Nickel of 0.2 %

Phosphorus

0.01 - 0.4 %

Show Material materials with Phosphorus of 0.01 - 0.4 %

Tin

5.5 - 7 %

Show Material materials with Tin of 5.5 - 7 %

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %