UNS C19210 boway

Alternative and trade names
boway 19210
Want to keep this datasheet? Save it now in your required format

Description

Excellent electrical conductivity and thermal conductivity combined with good softening resistance. It has medium strength and excellent bending formability as well as good corrosion resistance and good plating property. No sensitivity to stress corrosion cracking.

Equivalent Materials

This material data has been provided by Ningbo Boway Alloy Material.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValue

Density

8.9 g/cm³

Show Supplier Material materials with Density of 8.9 g/cm³

Dimension

PropertyValue

Dimensions

Strip thickness 0.08 - 3.0 mm, other gauges on request. Strip width from 8.5 mm. Hot-dip tinned and electroplated strip available.

Mechanical

PropertyValueTesting StandardComment

Bendability 180°, bw

1.5 [-]

Show Supplier Material materials with Bendability 180°, bw of 1.5 [-]

ASTM B820

R360(3/4H) | bending thickness: ≤ 0.5 mm & bending width: 10 mm

1.5 [-]

Show Supplier Material materials with Bendability 180°, bw of 1.5 [-]

ASTM B820

R385(H) | bending thickness: ≤ 0.5 mm & bending width: 10 mm

2 [-]

Show Supplier Material materials with Bendability 180°, bw of 2 [-]

ASTM B820

R415(EH) | bending thickness: ≤ 0.5 mm & bending width: 10 mm

2 [-]

Show Supplier Material materials with Bendability 180°, bw of 2 [-]

ASTM B820

R440(SH) | bending thickness: ≤ 0.5 mm & bending width: 10 mm

Bendability 180°, gw

1 [-]

Show Supplier Material materials with Bendability 180°, gw of 1 [-]

ASTM B820

R360(3/4H) | bending thickness: ≤ 0.5 mm & bending width: 10 mm

1.5 [-]

Show Supplier Material materials with Bendability 180°, gw of 1.5 [-]

ASTM B820

R385(H) | bending thickness: ≤ 0.5 mm & bending width: 10 mm

1.5 [-]

Show Supplier Material materials with Bendability 180°, gw of 1.5 [-]

ASTM B820

R415(EH) | bending thickness: ≤ 0.5 mm & bending width: 10 mm

2 [-]

Show Supplier Material materials with Bendability 180°, gw of 2 [-]

ASTM B820

R440(SH) | bending thickness: ≤ 0.5 mm & bending width: 10 mm

Bendability 90°, bw

1 [-]

Show Supplier Material materials with Bendability 90°, bw of 1 [-]

EN ISO 7438

R360(3/4H) | bending thickness: ≤ 0.5 mm & bending width: 10 mm

1 [-]

Show Supplier Material materials with Bendability 90°, bw of 1 [-]

EN ISO 7438

R385(H) | bending thickness: ≤ 0.5 mm & bending width: 10 mm

1.5 [-]

Show Supplier Material materials with Bendability 90°, bw of 1.5 [-]

EN ISO 7438

R415(EH) | bending thickness: ≤ 0.5 mm & bending width: 10 mm

2 [-]

Show Supplier Material materials with Bendability 90°, bw of 2 [-]

EN ISO 7438

R440(SH) | bending thickness: ≤ 0.5 mm & bending width: 10 mm

Bendability 90°, gw

0.5 [-]

Show Supplier Material materials with Bendability 90°, gw of 0.5 [-]

EN ISO 7438

R360(3/4H) | bending thickness: ≤ 0.5 mm & bending width: 10 mm

1 [-]

Show Supplier Material materials with Bendability 90°, gw of 1 [-]

EN ISO 7438

R385(H) | bending thickness: ≤ 0.5 mm & bending width: 10 mm

1.5 [-]

Show Supplier Material materials with Bendability 90°, gw of 1.5 [-]

EN ISO 7438

R415(EH) | bending thickness: ≤ 0.5 mm & bending width: 10 mm

1.5 [-]

Show Supplier Material materials with Bendability 90°, gw of 1.5 [-]

EN ISO 7438

R440(SH) | bending thickness: ≤ 0.5 mm & bending width: 10 mm

Elastic modulus

125 GPa

Show Supplier Material materials with Elastic modulus of 125 GPa

Elongation

1 %

Show Supplier Material materials with Elongation of 1 %

min. | R440(SH), A50

2 %

Show Supplier Material materials with Elongation of 2 %

min. | R415(EH), A50

3 %

Show Supplier Material materials with Elongation of 3 %

min. | R385(H), A50

4 %

Show Supplier Material materials with Elongation of 4 %

min. | R360(3/4H), A50

Hardness, Vickers

115 - 135 [-]

Show Supplier Material materials with Hardness, Vickers of 115 - 135 [-]

R360(3/4H) | For reference only

120 - 140 [-]

Show Supplier Material materials with Hardness, Vickers of 120 - 140 [-]

R385(H) | For reference only.

125 - 145 [-]

Show Supplier Material materials with Hardness, Vickers of 125 - 145 [-]

R415(EH) | For reference only

130 - 150 [-]

Show Supplier Material materials with Hardness, Vickers of 130 - 150 [-]

R440(SH) | For reference only

Poisson's ratio

0.33 [-]

Show Supplier Material materials with Poisson's ratio of 0.33 [-]

Tensile strength

360 - 425 MPa

Show Supplier Material materials with Tensile strength of 360 - 425 MPa

R360(3/4H)

385 - 455 MPa

Show Supplier Material materials with Tensile strength of 385 - 455 MPa

R385(H)

415 - 480 MPa

Show Supplier Material materials with Tensile strength of 415 - 480 MPa

R415(EH)

440 - 510 MPa

Show Supplier Material materials with Tensile strength of 440 - 510 MPa

R440(SH)

Yield strength

345 MPa

Show Supplier Material materials with Yield strength of 345 MPa

min. | R360(3/4H)

355 MPa

Show Supplier Material materials with Yield strength of 355 MPa

min. | R385(H)

400 MPa

Show Supplier Material materials with Yield strength of 400 MPa

min. | R415(EH)

425 MPa

Show Supplier Material materials with Yield strength of 425 MPa

min. | R440(SH)

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

1.7e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.7e-05 1/K

average value between 20-300°C

Specific heat capacity

385 J/(kg·K)

Show Supplier Material materials with Specific heat capacity of 385 J/(kg·K)

Thermal conductivity

20 °C

350 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 350 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical conductivity

20 °C

0.089 S/m

Show Supplier Material materials with Electrical conductivity of 0.089 S/m

Specific Electrical conductivity

20 °C

51 % IACS

Show Supplier Material materials with Specific Electrical conductivity of 51 % IACS

Chemical properties

PropertyValue

Copper

Balance

Iron

0.1 %

Show Supplier Material materials with Iron of 0.1 %

Phosphorus

0.03 %

Show Supplier Material materials with Phosphorus of 0.03 %

Technological properties

Property
Application areas

Application target:

Signal ConnectorSuitable
Power ConnectorSuitable
Miniaturized ConnectorNot recommended
Switch / RelaySuitable
SemiconductorGood


Ideal for semiconductor.

Chemical composition

The chemical composition is the nominal composition of the alloy

Coating

Electroplating: Good


Hot dip tinning: Very good

Cold Forming

Good

Machining

Fair

Packaging size

Standard coils with outside diameters up to 1300 mm. Traverse-wound coils with drum weights up to 500 kg. Multiple-coil up to 3 tons.

Testings

Fatigue strength:

The fatigue strength is defined as the maximum bending stress amplitude which a material withstands for 10.000.000 load cycles under symmetrical alternate load without breaking. It depends on the temper selected and can be estimated typically by 1/3 of tensile strength. For solid solution fine grain materials fatigue strength might increase up to 0,5 * of tensile strength.


Bending test:

90° bend test According to EN ISO 7438, 180° bend test acc. to ASTM B820, shown values might show orange- peel, however no crack.

Welding

Laser welding: Average


Resistance welding: Good