UNS C18160 boway

Alternative and trade names
boway 18160
Want to keep this datasheet? Save it now in your required format

Description

High electrical conductivity and thermal conductivity combined with medium strength and improved bending formability. Excellent stress relaxation and softening resistance.

Equivalent Materials

This material data has been provided by Ningbo Boway Alloy Material.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValue

Density

8.9 g/cm³

Show Supplier Material materials with Density of 8.9 g/cm³

Dimension

PropertyValue

Dimensions

Strip thickness 0.08 - 3.0 mm, other gauges on request. Strip width from 8.5 mm. Electroplated and Hot-dip tinned strip available.

Mechanical

PropertyValueTesting StandardComment

Bendability 180°, bw

1 [-]

Show Supplier Material materials with Bendability 180°, bw of 1 [-]

ASTM B820

R480 | bending thickness ≤ 0.5 mm & bending width: 10 mm

2.5 [-]

Show Supplier Material materials with Bendability 180°, bw of 2.5 [-]

ASTM B820

R540 | bending thickness ≤ 0.5 mm & bending width: 10 mm

Bendability 180°, gw

1 [-]

Show Supplier Material materials with Bendability 180°, gw of 1 [-]

ASTM B820

R480 | bending thickness ≤ 0.5 mm & bending width: 10 mm

2 [-]

Show Supplier Material materials with Bendability 180°, gw of 2 [-]

ASTM B820

R540 | bending thickness ≤ 0.5 mm & bending width: 10 mm

Bendability 90°, bw

0.5 [-]

Show Supplier Material materials with Bendability 90°, bw of 0.5 [-]

EN ISO 7438

R480 | bending thickness ≤ 0.5 mm & bending width: 10 mm

1 [-]

Show Supplier Material materials with Bendability 90°, bw of 1 [-]

EN ISO 7438

R540 | bending thickness ≤ 0.5 mm & bending width: 10 mm

Bendability 90°, gw

0.5 [-]

Show Supplier Material materials with Bendability 90°, gw of 0.5 [-]

EN ISO 7438

R480 | bending thickness ≤ 0.5 mm & bending width: 10 mm

1 [-]

Show Supplier Material materials with Bendability 90°, gw of 1 [-]

EN ISO 7438

R540 | bending thickness ≤ 0.5 mm & bending width: 10 mm

Elastic modulus

135 GPa

Show Supplier Material materials with Elastic modulus of 135 GPa

Elongation

4 %

Show Supplier Material materials with Elongation of 4 %

min. | R540, A50

8 %

Show Supplier Material materials with Elongation of 8 %

min. | R480, A50

Hardness, Vickers

150 - 190 [-]

Show Supplier Material materials with Hardness, Vickers of 150 - 190 [-]

R480 | For reference only

160 - 200 [-]

Show Supplier Material materials with Hardness, Vickers of 160 - 200 [-]

R540 | For reference only

Poisson's ratio

0.33 [-]

Show Supplier Material materials with Poisson's ratio of 0.33 [-]

Tensile strength

480 - 570 MPa

Show Supplier Material materials with Tensile strength of 480 - 570 MPa

R480

540 - 630 MPa

Show Supplier Material materials with Tensile strength of 540 - 630 MPa

R540

Yield strength

450 MPa

Show Supplier Material materials with Yield strength of 450 MPa

min. | R480

500 MPa

Show Supplier Material materials with Yield strength of 500 MPa

min. | R540

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

1.86e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.86e-05 1/K

average value between 20-300°C

Specific heat capacity

381 J/(kg·K)

Show Supplier Material materials with Specific heat capacity of 381 J/(kg·K)

Thermal conductivity

20 °C

340 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 340 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical conductivity

20 °C

0.088 S/m

Show Supplier Material materials with Electrical conductivity of 0.088 S/m

Specific Electrical conductivity

20 °C

51 % IACS

Show Supplier Material materials with Specific Electrical conductivity of 51 % IACS

Chemical properties

PropertyValue

Chromium

0.7 %

Show Supplier Material materials with Chromium of 0.7 %

Copper

Balance

Zirconium

0.1 %

Show Supplier Material materials with Zirconium of 0.1 %

Technological properties

Property
Application areas

Application target:

Signal ConnectorSuitable
Power ConnectorVery suitable
Miniaturized ConnectorSuitable
Switch / RelaySuitable
SemiconductorAverage


Ideal for power connectors.

Chemical composition

The chemical composition is the nominal composition of the alloy

Coating

Electroplating: Average


Hot dip tinning: Average

Cold Forming

Good

Machining

Not suitable

Packaging size

Standard coils with outside diameters up to 1200 mm. Traverse-wound coils with drum weights up to 500 kg. Multiple-coil up to 3 tons.

Soldering general

Soft soldering: Average

Testings

Fatigue strength:

The fatigue strength is defined as the maximum bending stress amplitude which a material withstands for 10.000.000 load cycles under symmetrical alternate load without breaking. It depends on the temper selected and can be estimated typically by 1/3 of tensile strength. For solid solution fine grain materials fatigue strength might increase up to 0,5 * of tensile strength.


Bending test:

90° bend test According to EN ISO 7438, 180° bend test acc. to ASTM B820, shown values might show orange- peel, however no crack.

Welding

Laser welding: Average


Resistance welding: Good