General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 1.27 g/cm³ Show Supplier Material materials with Density of 1.27 g/cm³ | ISO 1183 |
Limiting oxygen index | 23.0 °C | 47 % Show Supplier Material materials with Limiting oxygen index of 47 % | |
Moisture absorption | 23.0 °C | 0.7 % Show Supplier Material materials with Moisture absorption of 0.7 % | ISO 62 | (23°C / 50% RH) |
Water absorption | 23.0 °C | 1.25 % Show Supplier Material materials with Water absorption of 1.25 % | ISO 62-1 | (23°C/saturated) |
Mechanical
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Elastic modulus | 23.0 °C | 32 GPa Show Supplier Material materials with Elastic modulus of 32 GPa | ISO 527 | 1 mm/min | ||
Elongation | 23.0 °C | 6 % Show Supplier Material materials with Elongation of 6 % | ISO 527 | yield, 50 mm/min | ||
Flexural modulus | 23.0 °C | 3.3 GPa Show Supplier Material materials with Flexural modulus of 3.3 GPa | ISO 178 | 2 mm/min | ||
Flexural strength | 23.0 °C | 160 MPa Show Supplier Material materials with Flexural strength of 160 MPa | ISO 178 | yield, 2 mm/min | ||
Hardness, Ball Indentation | 23.0 °C | 140 MPa Show Supplier Material materials with Hardness, Ball Indentation of 140 MPa | ISO 2039-1 | H358/30 | ||
Hardness, Rockwell M | 23.0 °C | 109 [-] Show Supplier Material materials with Hardness, Rockwell M of 109 [-] | ASTM D 785 | | ||
Impact strength, Izod notched | 23.0 °C | 5 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 5 kJ/m² | ISO 180/1A | 80*10*4, 23°C | ||
Taber Abrasion | 23.0 °C | 10 mg/1000cy Show Supplier Material materials with Taber Abrasion of 10 mg/1000cy | ASTM D 1044 | CS-17, 1 kg | ||
Tensile strength | 23.0 °C | 105 MPa Show Supplier Material materials with Tensile strength of 105 MPa | ISO 527 | yield, 50 mm/min | ||
Impact strength, Izod unnotched | ISO 180/1U | unnotched 80*10*4, 23°C |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 5E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 5E-5 1/K | ISO 11359-2 | 23°C to 150°C |
Coefficient of thermal expansion, transverse | 23.0 °C | 5E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion, transverse of 5E-5 1/K | ISO 11359-2 | 23°C to 150°C |
Heat deflection temperature | 190 - 200 °C Show Supplier Material materials with Heat deflection temperature of 190 - 200 °C | ||
Heat deflection temperature, 0.45 MPa | 200 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 200 °C | ISO 75/Be | Edgew 120*10*4 sp=100mm | |
Heat deflection temperature, 1.80 MPa | 190 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 190 °C | ISO 75/Ae | Edgew 120*10*4 sp=100mm | |
Thermal conductivity | 23.0 °C | 0.24 W/(m·K) Show Supplier Material materials with Thermal conductivity of 0.24 W/(m·K) | ISO 8302 |
Vicat softening temperature | 211 °C Show Supplier Material materials with Vicat softening temperature of 211 °C | ISO 306 | Rate B/50 |
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Dielectric constant, 1MHz | 23.0 °C | 2.9 [-] Show Supplier Material materials with Dielectric constant, 1MHz of 2.9 [-] | IEC 60250 |
Dielectric constant, 60Hz | 23.0 °C | 2.9 [-] Show Supplier Material materials with Dielectric constant, 60Hz of 2.9 [-] | IEC 60250 | 50/60 Hz |
Dielectric strength | 23.0 °C | 16 kV/mm Show Supplier Material materials with Dielectric strength of 16 kV/mm | IEC 60243-1 | in oil, 3.2 mm, |
Dissipation factor | 23.0 °C | 2.5E-3 [-] Show Supplier Material materials with Dissipation factor of 2.5E-3 [-] | IEC 60250 | 2450 MHz |
Dissipation factor, 1MHz | 23.0 °C | 6E-3 [-] Show Supplier Material materials with Dissipation factor, 1MHz of 6E-3 [-] | IEC 60250 |
Dissipation factor, 50Hz | 23.0 °C | 5E-4 [-] Show Supplier Material materials with Dissipation factor, 50Hz of 5E-4 [-] | IEC 60250 | 50/60 Hz |
Volume resistivity | 23.0 °C | 1.00E+15 Ω·cm Show Supplier Material materials with Volume resistivity of 1.00E+15 Ω·cm | IEC 60093 | |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Melt volume-flow rate | 25 cm³/10min Show Supplier Material materials with Melt volume-flow rate of 25 cm³/10min | ISO 1133 | MVR at 360°C/5.0 kg | |
Shrinkage | 23.0 °C | 0.5 % Show Supplier Material materials with Shrinkage of 0.5 % | SABIC method | on tensile bar |
Technological properties
Property | ||
---|---|---|
Application areas | Circuit Board, Composite, Adhesives, Coating | |
Availability | Europe | |
Processing methods | Drying Temperature: 150°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |