General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 1.61 g/cm³ Show Supplier Material materials with Density of 1.61 g/cm³ | ASTM D 792 |
Moisture absorption | 23.0 °C | 0.04 % Show Supplier Material materials with Moisture absorption of 0.04 % | ISO 62 | (23°C / 50% RH) |
Relative density | 23.0 °C | 1.62 [-] Show Supplier Material materials with Relative density of 1.62 [-] | ASTM D 792 | |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 13.8 GPa Show Supplier Material materials with Elastic modulus of 13.8 GPa | ISO 527 | 1 mm/min |
Elongation | 23.0 °C | 2 % Show Supplier Material materials with Elongation of 2 % | ISO 527 | break, 5 mm/min |
Flexural modulus | 23.0 °C | 12.7 GPa Show Supplier Material materials with Flexural modulus of 12.7 GPa | ISO 178 | 2 mm/min |
Flexural strength | 23.0 °C | 265 MPa Show Supplier Material materials with Flexural strength of 265 MPa | ISO 178 | 2 mm/min |
Impact strength, Charpy notched | 23.0 °C | 12 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 12 kJ/m² | ISO 179/1eA | V-notch Edgew 80*10*4 sp=62mm, 23°C |
Impact strength, Izod notched | 23.0 °C | 12 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 12 kJ/m² | ISO 180/1A | 80*10*4, 23°C |
Impact strength, Izod notched, ASTM | 23.0 °C | 134 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 134 J/m | ASTM D 256 | notched, 23°C |
Impact strength, Izod unnotched | 23.0 °C | 58 kJ/m² Show Supplier Material materials with Impact strength, Izod unnotched of 58 kJ/m² | ISO 180/1U | unnotched 80*10*4 |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 873 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 873 J/m | ASTM D 4812 | 23°C |
Tensile strength | 23.0 °C | 193 MPa Show Supplier Material materials with Tensile strength of 193 MPa | ISO 527 | break, 5 mm/min |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 1.9E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.9E-5 1/K | ASTM E 831 | -40°C to 120°C |
Coefficient of thermal expansion, transverse | 23.0 °C | 3.7E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion, transverse of 3.7E-5 1/K | ASTM E 831 | -40°C to 120°C |
Heat deflection temperature | 310 - 336 °C Show Supplier Material materials with Heat deflection temperature of 310 - 336 °C | ||
Heat deflection temperature, 0.45 MPa | 336 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 336 °C | ISO 75/Bf | Flatw 80*10*4 sp=64mm | |
Heat deflection temperature, 1.80 MPa | 310 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 310 °C | ISO 75/Af | Flatw 80*10*4 sp=64mm |
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Dielectric constant | 23.0 °C | 4.03 [-] Show Supplier Material materials with Dielectric constant of 4.03 [-] | SABIC method | 1.9 GHz |
Dielectric constant, 1GHz | 23.0 °C | 4.02 [-] Show Supplier Material materials with Dielectric constant, 1GHz of 4.02 [-] | SABIC method | 1.1 GHz |
Dissipation factor | 23.0 °C | 4.5E-3 [-] Show Supplier Material materials with Dissipation factor of 4.5E-3 [-] | SABIC method |
Dissipation factor, 1GHz | 23.0 °C | 4.2E-3 [-] Show Supplier Material materials with Dissipation factor, 1GHz of 4.2E-3 [-] | SABIC method | |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Air Cabin Interiors, Heavy Vehicles, Enclosures, Electronic Components, Oil/Gas | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 120 to 150.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |