General
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 2.7 GPa Show Supplier Material materials with Elastic modulus of 2.7 GPa | ASTM D 638 | 50 mm/min |
Elongation | 23.0 °C | 12 % Show Supplier Material materials with Elongation of 12 % | ASTM D 638 | break, 6.35 mm |
Flexural modulus | 23.0 °C | 2.3 GPa Show Supplier Material materials with Flexural modulus of 2.3 GPa | ASTM D 790 | 6.4 mm |
Flexural strength | 23.0 °C | 70 MPa Show Supplier Material materials with Flexural strength of 70 MPa | ASTM D 790 | yield, 6.4 mm |
Instrumented Impact, at Peak | 23.0 °C | 29 J Show Supplier Material materials with Instrumented Impact, at Peak of 29 J | ASTM D 3763 | 23°C |
Tensile strength | 23.0 °C | 36 MPa Show Supplier Material materials with Tensile strength of 36 MPa | ASTM D 638 | yield, 6.35 mm |
Thermal
Property | Value | Comment | |
---|---|---|---|
Heat deflection temperature | 82 - 93 °C Show Supplier Material materials with Heat deflection temperature of 82 - 93 °C | ||
Heat deflection temperature, 0.45 MPa | 93 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 93 °C | ASTM D 648 | 6.4 mm, unannealed | |
Heat deflection temperature, 1.80 MPa | 82 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 82 °C | ASTM D 648 | 6.4 mm, unannealed | |
Relative temperature index, electrical | 65 °C Show Supplier Material materials with Relative temperature index, electrical of 65 °C | UL 746B | |
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | UL 746B | |
Relative temperature index, mechanical strength | 65 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C | UL 746B | |
Flammability | UL Recognized, 94V-1 Flame Class Rating: ≥3mm UL 94 <br> UL Recognized, 94-5VA Flame Class Rating: ≥3.9mm UL 94 <br> UL Recognized, 94V-0 Flame Class Rating: ≥6mm UL 94 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=101920328- - |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Melt volume-flow rate | 36 cm³/10min Show Supplier Material materials with Melt volume-flow rate of 36 cm³/10min | ISO 1133 | MVR at 280°C/5.0 kg | |
Shrinkage | 23.0 °C | 0.5 % Show Supplier Material materials with Shrinkage of 0.5 % | SABIC method | 6.4 mm |
Technological properties
Property | ||
---|---|---|
Application areas | Lab Ware and Clinical Diagnostics, Medical Device, Monitoring and Imaging | |
Availability | Europe,Asia,Americas | |
Processing methods | Front Temperature: 270 to 305.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |