LNP™ THERMOCOMP™ Compound ECF62

Want to keep this datasheet? Save it now in your required format

Description

LNP THERMOCOMP ECF62 is a compound based on Polyetherimide resin containing 30% Glass Fiber, 10% Carbon Fiber. Added features of this material include: Electrically Conductive.

This material data has been provided by Sabic.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.57 g/cm³

Show Supplier Material materials with Density of 1.57 g/cm³

ASTM D 792

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

17.9 GPa

Show Supplier Material materials with Elastic modulus of 17.9 GPa

ASTM D 638 | 50 mm/min

Elongation

23.0 °C

1.5 %

Show Supplier Material materials with Elongation of 1.5 %

ASTM D 638 | break

Flexural modulus

23.0 °C

15.9 GPa

Show Supplier Material materials with Flexural modulus of 15.9 GPa

ASTM D 790

Flexural strength

23.0 °C

268 MPa

Show Supplier Material materials with Flexural strength of 268 MPa

ASTM D 790

Impact strength, Izod notched

23.0 °C

69 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 69 kJ/m²

ASTM D 256 | notched, 23°C

Impact strength, Izod notched, ASTM

23.0 °C

69 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 69 J/m

ASTM D 256 | notched, 23°C

Impact strength, Izod unnotched, ASTM

23.0 °C

485 J/m

Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 485 J/m

ASTM D 4812 | 23°C

Tensile strength

23.0 °C

185 MPa

Show Supplier Material materials with Tensile strength of 185 MPa

ASTM D 638 | break

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

2.52E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 2.52E-5 1/K

ASTM E 831 | -40°C to 40°C

Coefficient of thermal expansion, transverse

23.0 °C

2.34E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion, transverse of 2.34E-5 1/K

ASTM E 831 | -40°C to 40°C

Heat deflection temperature

212 °C

Show Supplier Material materials with Heat deflection temperature of 212 °C

Heat deflection temperature, 1.80 MPa

212 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 212 °C

ASTM D 648 | 3.2mm, unannealed

Electrical

PropertyTemperatureValueComment

Volume resistivity

23.0 °C

1.00E+10 - 1.00E+11 Ω·cm

Show Supplier Material materials with Volume resistivity of 1.00E+10 - 1.00E+11 Ω·cm

ASTM D 257

Rheological Properties

PropertyTemperatureValueComment

Shrinkage

23.0 °C

0.1 %

Show Supplier Material materials with Shrinkage of 0.1 %

ASTM D 955 | 24 hrs

Shrinkage, transverse

23.0 °C

0.3 %

Show Supplier Material materials with Shrinkage, transverse of 0.3 %

ASTM D 955 | 24 hrs

Technological properties

Property
Availability

Europe,Asia,Americas

Processing methods

Drying Time: 4 to 6.0hrs
Maximum Moisture Content: 0.02%
Melt Temperature: 360 to 400.0°C
Front - Zone 3 Temperature: 380 to 400.0°C
Middle - Zone 2 Temperature: 370 to 390.0°C
Rear - Zone 1 Temperature: 360 to 380.0°C
Mold Temperature: 140 to 180.0°C
Back Pressure: 0.3 to 0.7MPa
Drying Temperature: 150°C
Nozzle Temperature: 390 to 400.0°C
Screw speed (Circumferential speed): 0.2 to 0.3m/s
Vent Depth: 0.025 to 0.076mm

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.