LNP™ THERMOCOMP™ Compound CX05470

Want to keep this datasheet? Save it now in your required format

Description

LNP THERMOCOMP CX05470 is a compound based on Polystyrene resin containing 20% Glass Fiber.

This material data has been provided by Sabic.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.18 g/cm³

Show Supplier Material materials with Density of 1.18 g/cm³

ASTM D 792

Moisture absorption

23.0 °C

0.07 %

Show Supplier Material materials with Moisture absorption of 0.07 %

ISO 62 | (23°C / 50% RH)

Relative density

23.0 °C

1.18 [-]

Show Supplier Material materials with Relative density of 1.18 [-]

ASTM D 792

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

6.8 GPa

Show Supplier Material materials with Elastic modulus of 6.8 GPa

ISO 527 | 1 mm/min

Elongation

23.0 °C

1.1 %

Show Supplier Material materials with Elongation of 1.1 %

ISO 527 | break, 5 mm/min

Flexural modulus

23.0 °C

6.3 GPa

Show Supplier Material materials with Flexural modulus of 6.3 GPa

ISO 178 | 2 mm/min

Flexural strength

23.0 °C

85 MPa

Show Supplier Material materials with Flexural strength of 85 MPa

ISO 178 | 2 mm/min

Impact strength, Izod notched

23.0 °C

3 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 3 kJ/m²

ISO 180/1A | notched 80*10*4, 23°C

Impact strength, Izod notched, ASTM

23.0 °C

36 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 36 J/m

ASTM D 256

Impact strength, Izod unnotched

23.0 °C

9 kJ/m²

Show Supplier Material materials with Impact strength, Izod unnotched of 9 kJ/m²

ISO 180/1U | 80*10*4, 23°C

Impact strength, Izod unnotched, ASTM

23.0 °C

156 J/m

Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 156 J/m

ASTM D 4812 | 23°C

Instrumented Impact, Total Energy

23.0 °C

8 J

Show Supplier Material materials with Instrumented Impact, Total Energy of 8 J

ASTM D 3763 | 23°C

Tensile strength

23.0 °C

52 MPa

Show Supplier Material materials with Tensile strength of 52 MPa

ISO 527 | break, 5 mm/min

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

5.6E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 5.6E-5 1/K

ASTM D 696 | -30°C to 30°C

Coefficient of thermal expansion, transverse

23.0 °C

6.9E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion, transverse of 6.9E-5 1/K

ASTM D 696 | -30°C to 30°C

Heat deflection temperature

92 - 97 °C

Show Supplier Material materials with Heat deflection temperature of 92 - 97 °C

Heat deflection temperature, 0.45 MPa

97 °C

Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 97 °C

ISO 75/Bf | Flatw 80*10*4 sp=64mm

Heat deflection temperature, 1.80 MPa

92 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 92 °C

ISO 75/Af | Flatw 80*10*4 sp=64mm

Rheological Properties

PropertyTemperatureValueComment

Shrinkage

23.0 °C

0.1 %

Show Supplier Material materials with Shrinkage of 0.1 %

ASTM D 955 | 24 hrs

Shrinkage, transverse

23.0 °C

0.2 %

Show Supplier Material materials with Shrinkage, transverse of 0.2 %

ASTM D 955 | 24 hrs

Technological properties

Property
Application areas

Meter Water

Availability

Europe,Asia,Americas

Processing methods

Drying Temperature: 80°C
Drying Time: 4hrs
Melt Temperature: 250°C
Front - Zone 3 Temperature: 265 to 275.0°C
Middle - Zone 2 Temperature: 245 to 255.0°C
Rear - Zone 1 Temperature: 220 to 230.0°C
Mold Temperature: 40 to 65.0°C
Back Pressure: 0.2 to 0.3MPa
Screw Speed: 30 to 60.0rpm

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.