Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 1.26 g/cm³ Show Supplier Material materials with Density of 1.26 g/cm³ | ASTM D 792 |
Relative density | 23.0 °C | 1.26 [-] Show Supplier Material materials with Relative density of 1.26 [-] | ASTM D 792 |
Mechanical
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Elastic modulus | 23.0 °C | 2.5 GPa Show Supplier Material materials with Elastic modulus of 2.5 GPa | ISO 527 | 1 mm/min | ||
Elongation | 23.0 °C | 5.4 % Show Supplier Material materials with Elongation of 5.4 % | ISO 527 | break, 5 mm/min | ||
Flexural modulus | 23.0 °C | 2.4 GPa Show Supplier Material materials with Flexural modulus of 2.4 GPa | ISO 178 | 2 mm/min | ||
Flexural strength | 23.0 °C | 87 MPa Show Supplier Material materials with Flexural strength of 87 MPa | ISO 178 | 2 mm/min | ||
Impact strength, Izod notched | 23.0 °C | 12 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 12 kJ/m² | ISO 180/1A | 80*10*4, 23°C | ||
Impact strength, Izod notched, ASTM | 23.0 °C | 153 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 153 J/m | ASTM D 256 | notched, 23°C | ||
Impact strength, Izod unnotched | 23.0 °C | 116 kJ/m² Show Supplier Material materials with Impact strength, Izod unnotched of 116 kJ/m² | ISO 180/1U | 80*10*4, 23°C | ||
Tensile strength | 23.0 °C | 49 MPa Show Supplier Material materials with Tensile strength of 49 MPa | ISO 527 | break, 5 mm/min | ||
Impact strength, Izod unnotched, ASTM | ASTM D 4812 | 23°C |
Thermal
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 5.8E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 5.8E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Coefficient of thermal expansion, transverse | 23.0 °C | 6.4E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion, transverse of 6.4E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Heat deflection temperature | 129 - 138 °C Show Supplier Material materials with Heat deflection temperature of 129 - 138 °C | ||||
Heat deflection temperature, 0.45 MPa | 138 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 138 °C | ISO 75/Bf | Flatw 80*10*4 sp=64mm | |||
Heat deflection temperature, 1.80 MPa | 129 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 129 °C | ISO 75/Af | Flatw 80*10*4 sp=64mm | |||
Relative temperature index, electrical | 80 °C Show Supplier Material materials with Relative temperature index, electrical of 80 °C | UL 746B | |||
Relative temperature index, mechanical impact | 80 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 80 °C | UL 746B | |||
Relative temperature index, mechanical strength | 80 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 80 °C | UL 746B | |||
Flammability | UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=102158629- - <br> UL Recognized, 94V-0 Flame Class Rating: ≥2mm UL 94 <br> UL Recognized, 94V-1 Flame Class Rating: ≥1.6mm UL 94 |
Electrical
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Building Accessory | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 120°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |