General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 1.33 g/cm³ Show Supplier Material materials with Density of 1.33 g/cm³ | ASTM D 792 |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 6 GPa Show Supplier Material materials with Elastic modulus of 6 GPa | ISO 527 | 1 mm/min |
Elongation | 23.0 °C | 2.9 % Show Supplier Material materials with Elongation of 2.9 % | ISO 527 | break, 5 mm/min |
Flexural modulus | 23.0 °C | 5.4 GPa Show Supplier Material materials with Flexural modulus of 5.4 GPa | ASTM D 790 | 1.3 mm/min, 50 mm span |
Flexural strength | 23.0 °C | 147 MPa Show Supplier Material materials with Flexural strength of 147 MPa | ASTM D 790 | brk, 1.3 mm/min, 50 mm span |
Impact strength, Charpy notched | 23.0 °C | 16 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 16 kJ/m² | ISO 179/2C | 23°C |
Impact strength, Charpy unnotched | 23.0 °C | 48 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 48 kJ/m² | ISO 179/2C | 23°C |
Impact strength, Izod notched | 23.0 °C | 160 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 160 kJ/m² | ASTM D 256 | notched, 23°C |
Impact strength, Izod notched, ASTM | 23.0 °C | 160 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 160 J/m | ASTM D 256 | notched, 23°C |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 627 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 627 J/m | ASTM D 4812 | 23°C |
Tensile strength | 23.0 °C | 99 MPa Show Supplier Material materials with Tensile strength of 99 MPa | ISO 527 | break, 5 mm/min |
Thermal
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 2.5E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 2.5E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Coefficient of thermal expansion, transverse | 23.0 °C | 6E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion, transverse of 6E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Heat deflection temperature | 126 - 130 °C Show Supplier Material materials with Heat deflection temperature of 126 - 130 °C | ||||
Heat deflection temperature, 0.45 MPa | 130 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 130 °C | ASTM D 648 | 3.2 mm, unannealed | |||
Heat deflection temperature, 1.80 MPa | 126 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 126 °C | ASTM D 648 | 3.2mm, unannealed | |||
Relative temperature index, electrical | 80 °C Show Supplier Material materials with Relative temperature index, electrical of 80 °C | UL 746B | |||
Relative temperature index, mechanical impact | 80 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 80 °C | UL 746B | |||
Relative temperature index, mechanical strength | 80 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 80 °C | UL 746B | |||
Flammability | UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=102475264- - <br> UL Recognized, 94HB Flame Class Rating: 0.5mm UL 94 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Melt volume-flow rate | 10 cm³/10min Show Supplier Material materials with Melt volume-flow rate of 10 cm³/10min | ASTM D 1238 | MVR at 300°C/1.2 kg | |
Shrinkage | 23.0 °C | 0.3 % Show Supplier Material materials with Shrinkage of 0.3 % | SABIC method |
Shrinkage, transverse | 23.0 °C | 0.3 % Show Supplier Material materials with Shrinkage, transverse of 0.3 % | SABIC method |
Technological properties
Property | ||
---|---|---|
Application areas | Wireless Communications | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 110°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |