Description

Thermoplastic Polyimide Extem* XH1015 Resin. Also UL rating 94V0 at 1.5 and 3.0.

This material data has been provided by Sabic.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.31 g/cm³

Show Supplier Material materials with Density of 1.31 g/cm³

ISO 1183

Relative density

23.0 °C

1.31 [-]

Show Supplier Material materials with Relative density of 1.31 [-]

ASTM D 792 |

Water absorption

23.0 °C

2.3 %

Show Supplier Material materials with Water absorption of 2.3 %

ISO 62-1 | (23°C/saturated)

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

3.1 GPa

Show Supplier Material materials with Elastic modulus of 3.1 GPa

ISO 527 | 1 mm/min

Elongation

23.0 °C

7 %

Show Supplier Material materials with Elongation of 7 %

ISO 527 | break, 5 mm/min

Flexural modulus

23.0 °C

2.9 GPa

Show Supplier Material materials with Flexural modulus of 2.9 GPa

ISO 178 | 2 mm/min

Flexural strength

23.0 °C

120 MPa

Show Supplier Material materials with Flexural strength of 120 MPa

ISO 178 | yield, 2 mm/min

Impact strength, Izod notched

23.0 °C

4 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 4 kJ/m²

ISO 180/1A | notched 80*10*4, 23°C

Impact strength, Izod notched, ASTM

23.0 °C

43 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 43 J/m

ASTM D 256

Tensile strength

23.0 °C

101 MPa

Show Supplier Material materials with Tensile strength of 101 MPa

ISO 527 | yield, 5 mm/min

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

5E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 5E-5 1/K

ISO 11359-2 | 23°C to 150°C

Coefficient of thermal expansion, transverse

23.0 °C

5.1E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion, transverse of 5.1E-5 1/K

ISO 11359-2 | 23°C to 150°C

Heat deflection temperature

223 - 250 °C

Show Supplier Material materials with Heat deflection temperature of 223 - 250 °C

Heat deflection temperature, 0.45 MPa

250 °C

Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 250 °C

ASTM D 648 | 3.2 mm, unannealed

Heat deflection temperature, 1.80 MPa

223 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 223 °C

ISO 75/Af | Flatw 80*10*4 sp=64mm

Vicat softening temperature

247 °C

Show Supplier Material materials with Vicat softening temperature of 247 °C

ISO 306 | Rate B/120

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

125 V

Show Supplier Material materials with Comparative tracking index of 125 V

IEC 60112 |

Dielectric constant, 1KHz

23.0 °C

3.5 [-]

Show Supplier Material materials with Dielectric constant, 1KHz of 3.5 [-]

ASTM D 150

Dielectric constant, 1MHz

23.0 °C

3.4 [-]

Show Supplier Material materials with Dielectric constant, 1MHz of 3.4 [-]

ASTM D 150

Dielectric strength

23.0 °C

25 kV/mm

Show Supplier Material materials with Dielectric strength of 25 kV/mm

ASTM D 149 | in air, 1.6 mm

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

10 g/10min

Show Supplier Material materials with Melt mass-flow rate of 10 g/10min

ASTM D 1238 | 367°C/6.6 kgf

Shrinkage

23.0 °C

1 %

Show Supplier Material materials with Shrinkage of 1 %

SABIC method | 3.2 mm

Technological properties

Property
Application areas

Non-LED Lighting, Wireless Communications, Wearables, Circuit Protection, Data Transfer, Data Management, Electronic Components, Fluid Delivery

Availability

Europe,Asia,Americas

Processing methods

Mold Temperature: 160 to 200.0°C
Nozzle Temperature: 375 to 405.0°C
Vent Depth: 0.025 to 0.076mm
Front - Zone 3 Temperature: 380 to 410.0°C
Middle - Zone 2 Temperature: 370 to 400.0°C
Drying Temperature: 175°C
Maximum Moisture Content: 0.02%
Drying Time (Cumulative): 24hrs
Rear - Zone 1 Temperature: 360 to 385.0°C
Drying Time: 4 to 6.0hrs
Melt Temperature: 380 to 410.0°C
Shot to Cylinder Size: 40 to 70.0%
Intake (throat) temperature: 70 to 100.0°C
Back pressure (Plastic Pressure): 5 to 10.0MPa
Screw speed (Circumferential speed): <0.2m/s

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.