General
Property | Temperature | Value | Comment |
---|---|---|---|
Water absorption | 23.0 °C | 0.18 % Show Supplier Material materials with Water absorption of 0.18 % | ASTM D 570 | (23°C/24hrs) |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 6 GPa Show Supplier Material materials with Elastic modulus of 6 GPa | ASTM D 638 | 5 mm/min |
Elongation | 23.0 °C | 3.5 % Show Supplier Material materials with Elongation of 3.5 % | ASTM D 638 | brk, Type I, 5 mm/min |
Flexural modulus | 23.0 °C | 6.6 GPa Show Supplier Material materials with Flexural modulus of 6.6 GPa | ASTM D 790 | 2.6 mm/min, 100 mm span |
Flexural strength | 23.0 °C | 179 MPa Show Supplier Material materials with Flexural strength of 179 MPa | ASTM D 790 | brk, 2.6 mm/min, 100 mm span |
Impact strength, Izod notched | 23.0 °C | 32 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 32 kJ/m² | ASTM D 256 | notched, 23°C |
Tensile strength | 23.0 °C | 103 MPa Show Supplier Material materials with Tensile strength of 103 MPa | ASTM D 638 | brk, Type I, 5 mm/min |
Thermal
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 2.34E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 2.34E-5 1/K | ASTM E 831 | -20°C to 150°C | ||
Coefficient of thermal expansion, transverse | 23.0 °C | 2.7E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion, transverse of 2.7E-5 1/K | ASTM E 831 | -20°C to 150°C | ||
Heat deflection temperature | 207 °C Show Supplier Material materials with Heat deflection temperature of 207 °C | ||||
Heat deflection temperature, 1.80 MPa | 207 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 207 °C | ASTM D 648 | 6.4 mm, unannealed | |||
Relative temperature index, electrical | 170 °C Show Supplier Material materials with Relative temperature index, electrical of 170 °C | UL 746B | |||
Relative temperature index, mechanical impact | 170 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 170 °C | UL 746B | |||
Relative temperature index, mechanical strength | 170 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 170 °C | UL 746B | |||
Flammability | UL Recognized, 94V-0 Flame Class Rating: ≥0.81mm UL 94 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=221100- - <br> Glow Wire Flammability Index, 1.5 mm: 960°C IEC 60695-2-12 <br> Glow Wire Ignitability Temperature, 1.5 mm: 875°C IEC 60695-2-13 |
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Comparative tracking index | 23.0 °C | 4 V Show Supplier Material materials with Comparative tracking index of 4 V | UL 746A | (UL) {PLC} |
Dielectric constant, 1MHz | 23.0 °C | 3.49 [-] Show Supplier Material materials with Dielectric constant, 1MHz of 3.49 [-] | ASTM D 150 |
High Amp Arc Ignition | 23.0 °C | 0.81 mm Show Supplier Material materials with High Amp Arc Ignition of 0.81 mm | ≥, UL 746A | PLC 4 |
High Volt Arc Track Rate | 23.0 °C | 0 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 0 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 0.81 mm Show Supplier Material materials with Hot-Wire Ignition of 0.81 mm | ≥, UL 746A | PLC 2 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Shrinkage | 23.0 °C | 0.3 % Show Supplier Material materials with Shrinkage of 0.3 % | SABIC method | 3.2 mm |
Technological properties
Property | ||
---|---|---|
Application areas | Pump, Non-LED Lighting, Enclosures, Forward Lighting, Lab Ware and Clinical Diagnostics, Heavy Vehicles | |
Availability | Europe,Asia,Americas | |
Processing methods | Mold Temperature: 135 to 165.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |