General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 1.41 g/cm³ Show Supplier Material materials with Density of 1.41 g/cm³ | ASTM D 792 |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 14.9 GPa Show Supplier Material materials with Elastic modulus of 14.9 GPa | ASTM D 638 | 50 mm/min |
Elongation | 23.0 °C | 2.6 % Show Supplier Material materials with Elongation of 2.6 % | ASTM D 638 | break |
Flexural modulus | 23.0 °C | 14.4 GPa Show Supplier Material materials with Flexural modulus of 14.4 GPa | ASTM D 790 |
Flexural strength | 23.0 °C | 296 MPa Show Supplier Material materials with Flexural strength of 296 MPa | ASTM D 790 |
Impact strength, Izod notched | 23.0 °C | 85 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 85 kJ/m² | ASTM D 256 | notched, 23°C |
Impact strength, Izod notched, ASTM | 23.0 °C | 85 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 85 J/m | ASTM D 256 |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 807 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 807 J/m | ASTM D 4812 | 23°C |
Tensile strength | 23.0 °C | 171 MPa Show Supplier Material materials with Tensile strength of 171 MPa | ASTM D 638 | break |
Thermal
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Sheet resistivity, ROA | 23.0 °C | 10 - 1000000 Ω Show Supplier Material materials with Sheet resistivity, ROA of 10 - 1000000 Ω | ASTM D 257 |
Technological properties
Property | ||
---|---|---|
Availability | Asia,Americas | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |