General
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of friction | 0.59 [-] Show Supplier Material materials with Coefficient of friction of 0.59 [-] | ||
Coefficient of friction, kinetic | 0.59 [-] Show Supplier Material materials with Coefficient of friction, kinetic of 0.59 [-] | ASTM D 3702 Modified: Manual | |
Density | 23.0 °C | 1.51 g/cm³ Show Supplier Material materials with Density of 1.51 g/cm³ | ISO 1183 |
Moisture absorption | 23.0 °C | 0.46 % Show Supplier Material materials with Moisture absorption of 0.46 % | ISO 62 | (23°C / 50% RH) |
Water absorption | 23.0 °C | 1.34 % Show Supplier Material materials with Water absorption of 1.34 % | ISO 62-1 | (23°C/24hrs) |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elongation | 23.0 °C | 2.6 % Show Supplier Material materials with Elongation of 2.6 % | ISO 527 | break, 5 mm/min |
Flexural modulus | 23.0 °C | 7.2 GPa Show Supplier Material materials with Flexural modulus of 7.2 GPa | ISO 178 | 2 mm/min |
Flexural strain | 23.0 °C | 5.6 % Show Supplier Material materials with Flexural strain of 5.6 % | ISO 178 | break, 2 mm/min, 150°C |
Flexural strength | 23.0 °C | 234 MPa Show Supplier Material materials with Flexural strength of 234 MPa | ISO 178 | yield, 2 mm/min |
Impact strength, Izod notched | 23.0 °C | 16 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 16 kJ/m² | ISO 180/1A | 80*10*4, 23°C |
Impact strength, Izod unnotched | 23.0 °C | 74 kJ/m² Show Supplier Material materials with Impact strength, Izod unnotched of 74 kJ/m² | ISO 180/1U | unnotched 80*10*4, -40°C |
Tensile strength | 23.0 °C | 166 MPa Show Supplier Material materials with Tensile strength of 166 MPa | ISO 527 | break, 5 mm/min |
Thermal
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 2.5E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 2.5E-5 1/K | ISO 11359-2 | 23°C to 60°C | ||
Coefficient of thermal expansion, transverse | 23.0 °C | 7.5E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion, transverse of 7.5E-5 1/K | ISO 11359-2 | 23°C to 60°C | ||
Relative temperature index, electrical | 120 °C Show Supplier Material materials with Relative temperature index, electrical of 120 °C | UL 746B | |||
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | UL 746B | |||
Relative temperature index, mechanical strength | 65 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C | UL 746B | |||
Specific heat capacity | 23.0 °C | 1988 J/(kg·K) Show Supplier Material materials with Specific heat capacity of 1988 J/(kg·K) | ASTM E 1269 | ||
Thermal conductivity | 23.0 °C | 0.25 W/(m·K) Show Supplier Material materials with Thermal conductivity of 0.25 W/(m·K) | ASTM D 5930 | ||
Flammability | UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=101344610- - <br> UL Recognized, 94HB Flame Class Rating: ≥0.75mm UL 94 <br> UL Yellow Card Link 2: https://iq.ul.com/ul/cert.aspx?ULID=101282824- - <br> UL Yellow Card Link 3: https://iq.ul.com/ul/cert.aspx?ULID=101344595- - |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Melt volume-flow rate | 15 cm³/10min Show Supplier Material materials with Melt volume-flow rate of 15 cm³/10min | ISO 1133 | MVR at 275°C/5 kg | |
Shrinkage | 23.0 °C | 0.2 % Show Supplier Material materials with Shrinkage of 0.2 % | ISO 294 | 24 hrs |
Shrinkage, transverse | 23.0 °C | 0.8 % Show Supplier Material materials with Shrinkage, transverse of 0.8 % | ISO 294 | 24 hrs |
Technological properties
Property | ||
---|---|---|
Application areas | Document Handling, Data Transfer, Auto Aftermarket, ATM/Ticket Machine, Circuit Protection, Air Intake System, Lab Ware and Clinical Diagnostics, Engine Component, Engine Cooling System, Front Grille, Enclosures, Enclosure/Housing/Cover, Electronic Components, Personal Computing, Power Manangement, Pharmaceutical Packaging & Drug Delivery, Surgical Devices, Security/Detection, Wireless Communications, Wiring Devices | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 80°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |