NORYL™ Resin V0150B - Asia

Want to keep this datasheet? Save it now in your required format

Description

NORYL™ V0150B resin is a non-reinforced blend of polyphenylene ether (PPE) + high impact polystyrene (HIPS). This injection moldable contains non-brominated, non-chlorinated flame retardant and carries a UL94 flame rating of V0 at 1.5mm along with a UL746C Outdoor Suitability rating of F1. exhibits good low temperature impact resistance, damp heat performance, low moisture absorption and good dimensional stability. NORYL V0150B resin is an excellent candidate for parts that are exposed to tough outdoor environments, such as Solar / Photovoltaic (PV) junction boxes and outdoor housings and enclosures.

This material data has been provided by Sabic.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.11 g/cm³

Show Supplier Material materials with Density of 1.11 g/cm³

ISO 1183

Limiting oxygen index

23.0 °C

32 %

Show Supplier Material materials with Limiting oxygen index of 32 %

Moisture absorption

23.0 °C

0.06 %

Show Supplier Material materials with Moisture absorption of 0.06 %

ISO 62 | (23°C / 50% RH)

Relative density

23.0 °C

1.11 [-]

Show Supplier Material materials with Relative density of 1.11 [-]

ASTM D 792

Water absorption

23.0 °C

0.18 %

Show Supplier Material materials with Water absorption of 0.18 %

ISO 62-1 | (23°C/saturated)

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

2.5 GPa

Show Supplier Material materials with Elastic modulus of 2.5 GPa

ISO 527 | 1 mm/min

Elongation

23.0 °C

10 %

Show Supplier Material materials with Elongation of 10 %

ISO 527 | break, 50 mm/min

Flexural modulus

23.0 °C

2.4 GPa

Show Supplier Material materials with Flexural modulus of 2.4 GPa

ISO 178 | 2 mm/min

Flexural strength

23.0 °C

110 MPa

Show Supplier Material materials with Flexural strength of 110 MPa

ISO 178 | yield, 2 mm/min

Hardness, Ball Indentation

23.0 °C

113 MPa

Show Supplier Material materials with Hardness, Ball Indentation of 113 MPa

ISO 2039-1 | H358/30

Impact strength, Charpy notched

23.0 °C

14 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 14 kJ/m²

ISO 179/1eA | V-notch Edgew, 23°C, 80*10*4 sp=62mm

Impact strength, Izod notched

23.0 °C

5 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 5 kJ/m²

ISO 180/1A | notched 80*10*4, -30°C

Impact strength, Izod notched, ASTM

23.0 °C

180 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 180 J/m

ASTM D 256 | notched, -30°C

Instrumented Impact, Total Energy

23.0 °C

50 J

Show Supplier Material materials with Instrumented Impact, Total Energy of 50 J

ASTM D 3763 | 23°C

Taber Abrasion

23.0 °C

35 mg/1000cy

Show Supplier Material materials with Taber Abrasion of 35 mg/1000cy

SABIC method | CS-17, 1 kg

Tensile strength

23.0 °C

55 MPa

Show Supplier Material materials with Tensile strength of 55 MPa

ISO 527 | break, 50 mm/min

Thermal

PropertyTemperatureValueComment

Ball pressure temperature

140 °C

Show Supplier Material materials with Ball pressure temperature of 140 °C

IEC 60695-10-2 | approximate maximum

Coefficient of thermal expansion

23.0 °C

7E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 7E-5 1/K

ISO 11359-2 | 23°C to 80°C

Coefficient of thermal expansion, transverse

23.0 °C

9E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion, transverse of 9E-5 1/K

ISO 11359-2 | 23°C to 80°C

Glow Wire Flammability Index

960 °C

Show Supplier Material materials with Glow Wire Flammability Index of 960 °C

Glow Wire Ignition Temperature

775 °C

Show Supplier Material materials with Glow Wire Ignition Temperature of 775 °C

IEC 60695-2-13 | 3.0 mm

Heat deflection temperature

130 - 140 °C

Show Supplier Material materials with Heat deflection temperature of 130 - 140 °C

Heat deflection temperature, 0.45 MPa

140 °C

Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 140 °C

ISO 75/Be | Edgew 120*10*4 sp=100mm

Heat deflection temperature, 1.80 MPa

130 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 130 °C

ISO 75/Ae | Edgew 120*10*4 sp=100mm

Relative temperature index, electrical

110 °C

Show Supplier Material materials with Relative temperature index, electrical of 110 °C

UL 746B

Relative temperature index, mechanical impact

105 °C

Show Supplier Material materials with Relative temperature index, mechanical impact of 105 °C

UL 746B

Relative temperature index, mechanical strength

115 °C

Show Supplier Material materials with Relative temperature index, mechanical strength of 115 °C

UL 746B

Thermal conductivity

23.0 °C

0.27 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 0.27 W/(m·K)

ISO 8302

Vicat softening temperature

155 °C

Show Supplier Material materials with Vicat softening temperature of 155 °C

ISO 306 | Rate B/120

Flammability

Glow Wire Ignitability Temperature, 1.0 mm: 775°C IEC 60695-2-13 <br> UL Recognized, 94V-0 Flame Class Rating: ≥1mm UL 94 <br> UL Recognized, 94-5VA Flame Class Rating: ≥2mm UL 94 <br> Glow Wire Flammability Index, 1.0 mm: 960°C IEC 60695-2-12 <br> Glow Wire Flammability Index, 1.5 mm: 960°C IEC 60695-2-12 <br> Glow Wire Ignitability Temperature, 1.5 mm: 775°C IEC 60695-2-13 <br> UL Recognized, 94V-1 Flame Class Rating: ≥0.8mm UL 94 <br> UV-light, water exposure/immersion: F1- UL 746C <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=100727518- - <br> UL Yellow Card Link 2: https://iq.ul.com/ul/cert.aspx?ULID=100727519- -

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

2 V

Show Supplier Material materials with Comparative tracking index of 2 V

UL 746A | (UL) {PLC}

Dielectric constant, 1MHz

23.0 °C

2.7 [-]

Show Supplier Material materials with Dielectric constant, 1MHz of 2.7 [-]

IEC 60250

Dielectric constant, 60Hz

23.0 °C

2.8 [-]

Show Supplier Material materials with Dielectric constant, 60Hz of 2.8 [-]

IEC 60250 | 50/60 Hz

Dielectric strength

23.0 °C

16 kV/mm

Show Supplier Material materials with Dielectric strength of 16 kV/mm

IEC 60243-1 | in oil, 3.2 mm,

Dissipation factor, 1MHz

23.0 °C

3E-3 [-]

Show Supplier Material materials with Dissipation factor, 1MHz of 3E-3 [-]

IEC 60250

Dissipation factor, 50Hz

23.0 °C

9E-4 [-]

Show Supplier Material materials with Dissipation factor, 50Hz of 9E-4 [-]

IEC 60250 | 50/60 Hz

High Amp Arc Ignition

23.0 °C

0.8 mm

Show Supplier Material materials with High Amp Arc Ignition of 0.8 mm

≥, UL 746A | PLC 0

High Volt Arc Track Rate

23.0 °C

4 PLC Code

Show Supplier Material materials with High Volt Arc Track Rate of 4 PLC Code

UL 746A | (PLC)

Hot-Wire Ignition

23.0 °C

0.8 mm

Show Supplier Material materials with Hot-Wire Ignition of 0.8 mm

≥, UL 746A | PLC 0

Sheet resistivity, ROA

23.0 °C

1.00E+15 Ω

Show Supplier Material materials with Sheet resistivity, ROA of 1.00E+15 Ω

>, IEC 60093

Volume resistivity

23.0 °C

1.00E+15 Ω·cm

Show Supplier Material materials with Volume resistivity of 1.00E+15 Ω·cm

IEC 60093 |

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

3.5 g/10min

Show Supplier Material materials with Melt mass-flow rate of 3.5 g/10min

ASTM D 1238 | 280°C/5.0 kgf

Melt volume-flow rate

10 cm³/10min

Show Supplier Material materials with Melt volume-flow rate of 10 cm³/10min

ISO 1133 | MVR at 300°C/5.0 kg

Shrinkage

23.0 °C

0.5 %

Show Supplier Material materials with Shrinkage of 0.5 %

SABIC method | 3.2 mm

Technological properties

Property
Application areas

Pump, Photovoltaic Components, Plumbing, Non-LED Lighting, Personal Computing, Infrastructure, Medical Device, LED Lighting, Washing Machine, Wiring Devices, Wireless Communications, Coffee Maker/Espresso Machine, Document Handling, Dishwasher, Circuit Protection, Amusement Machine, Enclosure/Housing/Cover, Electronics, Energy Management, Enclosures, Electronic Components

Availability

Europe,Asia,Americas

Processing methods

Hopper Temperature: 80 to 100.0°C
Mold Temperature: 100 to 130.0°C
Drying Temperature: 110 to 120.0°C
Drying Time: 2 to 3.0hrs
Front - Zone 3 Temperature: 300 to 320.0°C
Rear - Zone 1 Temperature: 260 to 280.0°C
Melt Temperature: 300 to 320.0°C
Nozzle Temperature: 280 to 300.0°C
Middle - Zone 2 Temperature: 280 to 300.0°C

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.