NORYL™ Resin FP5140 - Europe

Want to keep this datasheet? Save it now in your required format

Description

NORYL™ FP5140 resin is a non-reinforced blend of polyphenylene ether (PPE) + high impact polystyrene (HIPS). This injection moldable grade contains non-brominated, non-chlorinated flame retardant with a UL94 flame rating of V1 at 1.5mm NORYL FP5140 resin was designed to have very good dimensional stability with high flow and exhibits good rheological properties, high heat resistance, hydrolysis resistance, and very low density. The combination of these properties makes this material an excellent candidate for Flat Panel TV enclosure applications.

This material data has been provided by Sabic.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.11 g/cm³

Show Supplier Material materials with Density of 1.11 g/cm³

ISO 1183

Limiting oxygen index

23.0 °C

30 %

Show Supplier Material materials with Limiting oxygen index of 30 %

Moisture absorption

23.0 °C

0.05 %

Show Supplier Material materials with Moisture absorption of 0.05 %

ISO 62 | (23°C / 50% RH)

Relative density

23.0 °C

1.11 [-]

Show Supplier Material materials with Relative density of 1.11 [-]

ASTM D 792

Water absorption

23.0 °C

0.18 %

Show Supplier Material materials with Water absorption of 0.18 %

ISO 62-1 | (23°C/saturated)

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

2.5 GPa

Show Supplier Material materials with Elastic modulus of 2.5 GPa

ISO 527 | 1 mm/min

Elongation

23.0 °C

3.5 %

Show Supplier Material materials with Elongation of 3.5 %

ISO 527 | yield, 50 mm/min

Flexural modulus

23.0 °C

2.3 GPa

Show Supplier Material materials with Flexural modulus of 2.3 GPa

ISO 178 | 2 mm/min

Flexural strength

23.0 °C

87 MPa

Show Supplier Material materials with Flexural strength of 87 MPa

ISO 178 | yield, 2 mm/min

Impact strength, Charpy notched

23.0 °C

5 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 5 kJ/m²

ISO 179/1eA | V-notch Edgew 80*10*4 sp=62mm, 23°C

Impact strength, Izod notched

23.0 °C

4 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 4 kJ/m²

ISO 180/1A | 80*10*4, -30°C

Tensile strength

23.0 °C

48 MPa

Show Supplier Material materials with Tensile strength of 48 MPa

ISO 527 | break, 50 mm/min

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

8.3E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 8.3E-5 1/K

ISO 11359-2 | -40°C to 40°C

Coefficient of thermal expansion, transverse

23.0 °C

7.7E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion, transverse of 7.7E-5 1/K

ISO 11359-2 | -40°C to 40°C

Glow Wire Ignition Temperature

725 °C

Show Supplier Material materials with Glow Wire Ignition Temperature of 725 °C

IEC 60695-2-13 | 3.0 mm

Heat deflection temperature

85 °C

Show Supplier Material materials with Heat deflection temperature of 85 °C

Heat deflection temperature, 1.80 MPa

85 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 85 °C

ISO 75/Af | Flatw 80*10*4 sp=64mm

Relative temperature index, electrical

65 °C

Show Supplier Material materials with Relative temperature index, electrical of 65 °C

UL 746B

Relative temperature index, mechanical impact

65 °C

Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C

UL 746B

Relative temperature index, mechanical strength

65 °C

Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C

UL 746B

Vicat softening temperature

110 °C

Show Supplier Material materials with Vicat softening temperature of 110 °C

ISO 306 | Rate B/120

Flammability

Glow Wire Flammability Index 960°C, passes at: 3mm IEC 60695-2-12 <br> Glow Wire Flammability Index 960°C, passes at: 3mm IEC 60695-2-12 <br> UL Recognized, 94V-0 Flame Class Rating: ≥2mm UL 94 <br> UL Recognized, 94V-1 Flame Class Rating: ≥1.5mm UL 94 <br> UL Recognized, 94V-2 Flame Class Rating: ≥1mm UL 94 <br> UL Recognized, 94V-2 Flame Class Rating: ≥1mm UL 94 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=644141- - <br> Glow Wire Ignitability Temperature, 1.0 mm: 700°C IEC 60695-2-13

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

250 V

Show Supplier Material materials with Comparative tracking index of 250 V

IEC 60112 |

Dielectric constant, 1MHz

23.0 °C

2.8 [-]

Show Supplier Material materials with Dielectric constant, 1MHz of 2.8 [-]

IEC 60250

Dielectric strength

23.0 °C

27.5 kV/mm

Show Supplier Material materials with Dielectric strength of 27.5 kV/mm

IEC 60243-1 | in oil, 1.6 mm

Dissipation factor, 1MHz

23.0 °C

2E-3 [-]

Show Supplier Material materials with Dissipation factor, 1MHz of 2E-3 [-]

IEC 60250

Sheet resistivity, ROA

23.0 °C

8.00E+16 - 8.50E+16 Ω

Show Supplier Material materials with Sheet resistivity, ROA of 8.00E+16 - 8.50E+16 Ω

IEC 60093

Volume resistivity

23.0 °C

3.00E+16 - 3.50E+16 Ω·cm

Show Supplier Material materials with Volume resistivity of 3.00E+16 - 3.50E+16 Ω·cm

IEC 60093

Rheological Properties

PropertyTemperatureValueComment

Melt volume-flow rate

15 cm³/10min

Show Supplier Material materials with Melt volume-flow rate of 15 cm³/10min

ISO 1133 | MVR at 280°C/1.2 kg

Shrinkage

23.0 °C

0.5 %

Show Supplier Material materials with Shrinkage of 0.5 %

SABIC method | 3.2 mm

Technological properties

Property
Application areas

Displays

Availability

Americas

Processing methods

Nozzle Temperature: 240 to 270.0°C
Hopper Temperature: 60 to 80.0°C
Drying Time: 2 to 3.0hrs
Drying Temperature: 70 to 80.0°C
Middle - Zone 2 Temperature: 230 to 260.0°C
Front - Zone 3 Temperature: 250 to 285.0°C
Rear - Zone 1 Temperature: 200 to 220.0°C
Mold Temperature: 40 to 65.0°C
Melt Temperature: 250 to 285.0°C

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.