General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 1.28 g/cm³ Show Supplier Material materials with Density of 1.28 g/cm³ | ISO 1183 |
Moisture absorption | 23.0 °C | 0.2 % Show Supplier Material materials with Moisture absorption of 0.2 % | ISO 62 | (23°C / 50% RH) |
Relative density | 23.0 °C | 1.28 [-] Show Supplier Material materials with Relative density of 1.28 [-] | ASTM D 792 |
Water absorption | 23.0 °C | 1.2 % Show Supplier Material materials with Water absorption of 1.2 % | ISO 62-1 | (23°C/saturated) |
Mechanical
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Elastic modulus | 23.0 °C | 2.9 GPa Show Supplier Material materials with Elastic modulus of 2.9 GPa | ISO 527 | 1 mm/min | ||
Elongation | 23.0 °C | 8 % Show Supplier Material materials with Elongation of 8 % | ISO 527 | yield, 5 mm/min | ||
Flexural modulus | 23.0 °C | 2.9 GPa Show Supplier Material materials with Flexural modulus of 2.9 GPa | ISO 178 | 2 mm/min | ||
Flexural strength | 23.0 °C | 110 MPa Show Supplier Material materials with Flexural strength of 110 MPa | ISO 178 | yield, 2 mm/min | ||
Impact strength, Charpy notched | 23.0 °C | 7 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 7 kJ/m² | ISO 179/1eA | V-notch Edgew, 23°C, 80*10*4 sp=62mm | ||
Impact strength, Izod notched | 23.0 °C | 5 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 5 kJ/m² | ISO 180/1A | notched 80*10*4, -30°C | ||
Impact strength, Izod notched, ASTM | 23.0 °C | 59 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 59 J/m | ASTM D 256 | notched, 23°C | ||
Impact strength, Izod unnotched, ASTM | 23.0 °C | 2100 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 2100 J/m | ASTM D 4812 | 23°C | ||
Instrumented Impact, Total Energy | 23.0 °C | 30 J Show Supplier Material materials with Instrumented Impact, Total Energy of 30 J | ASTM D 3763 | 23°C | ||
Tensile strength | 23.0 °C | 85 MPa Show Supplier Material materials with Tensile strength of 85 MPa | ISO 527 | break, 5 mm/min | ||
Impact strength, Charpy unnotched | ISO 179/1eU | Unnotch Edgew 80*10*4 sp=62mm, -30°C | ||||
Impact strength, Izod unnotched | ISO 180/1U | unnotched 80*10*4, -30°C |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Ball Pressure Test | Passes | IEC 60695-10-2 | 125°C +/- 2°C | |
Coefficient of thermal expansion | 23.0 °C | 5.5E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 5.5E-5 1/K | ISO 11359-2 | 23°C to 150°C |
Coefficient of thermal expansion, transverse | 23.0 °C | 5.5E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion, transverse of 5.5E-5 1/K | ISO 11359-2 | 23°C to 150°C |
Heat deflection temperature | 198 - 208 °C Show Supplier Material materials with Heat deflection temperature of 198 - 208 °C | ||
Heat deflection temperature, 0.45 MPa | 208 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 208 °C | ISO 75/Bf | Flatw 80*10*4 sp=64mm | |
Heat deflection temperature, 1.80 MPa | 198 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 198 °C | ISO 75/Af | Flatw 80*10*4 sp=64mm | |
Thermal conductivity | 23.0 °C | 0.31 W/(m·K) Show Supplier Material materials with Thermal conductivity of 0.31 W/(m·K) | ASTM C177 |
Vicat softening temperature | 220 °C Show Supplier Material materials with Vicat softening temperature of 220 °C | ISO 306 | Rate A/50 |
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Comparative tracking index | 23.0 °C | 100 V Show Supplier Material materials with Comparative tracking index of 100 V | IEC 60112 | M |
Dielectric constant, 60Hz | 23.0 °C | 3.2 [-] Show Supplier Material materials with Dielectric constant, 60Hz of 3.2 [-] | ASTM D 150 | 50/60 Hz |
Dielectric strength | 23.0 °C | 18.1 kV/mm Show Supplier Material materials with Dielectric strength of 18.1 kV/mm | IEC 60243-1 | in oil, 3.2 mm, |
Dissipation factor, 50Hz | 23.0 °C | 2.1E-3 [-] Show Supplier Material materials with Dissipation factor, 50Hz of 2.1E-3 [-] | IEC 60250 | 50/60 Hz |
Sheet resistivity, ROA | 23.0 °C | 1.00E+15 Ω Show Supplier Material materials with Sheet resistivity, ROA of 1.00E+15 Ω | >, IEC 60093 |
Volume resistivity | 23.0 °C | 2.50E+15 Ω·cm Show Supplier Material materials with Volume resistivity of 2.50E+15 Ω·cm | IEC 60093 | |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Melt mass-flow rate | 11 g/10min Show Supplier Material materials with Melt mass-flow rate of 11 g/10min | ASTM D 1238 | 337°C/6.6 kgf | |
Melt volume-flow rate | 20 cm³/10min Show Supplier Material materials with Melt volume-flow rate of 20 cm³/10min | ISO 1133 | MVR at 360°C/5.0 kg | |
Shrinkage | 23.0 °C | 0.4 % Show Supplier Material materials with Shrinkage of 0.4 % | SABIC method | 3.2 mm |
Shrinkage, transverse | 23.0 °C | 0.4 % Show Supplier Material materials with Shrinkage, transverse of 0.4 % | SABIC method | 3.2 mm |
Technological properties
Property | ||
---|---|---|
Application areas | Electronic Components | |
Availability | Europe,Asia,Americas | |
Processing methods | Mold Temperature: 135 to 165.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |