Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 1.46 g/cm³ Show Supplier Material materials with Density of 1.46 g/cm³ | ISO 1183 |
Moisture absorption | 23.0 °C | 0.12 % Show Supplier Material materials with Moisture absorption of 0.12 % | ISO 62 | (23°C / 50% RH) |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 9.1 GPa Show Supplier Material materials with Elastic modulus of 9.1 GPa | ISO 527 | 1 mm/min |
Elongation | 23.0 °C | 2 % Show Supplier Material materials with Elongation of 2 % | ISO 527 | break, 5 mm/min |
Flexural modulus | 23.0 °C | 8.5 GPa Show Supplier Material materials with Flexural modulus of 8.5 GPa | ISO 178 | 2 mm/min |
Flexural strength | 23.0 °C | 196 MPa Show Supplier Material materials with Flexural strength of 196 MPa | ASTM D 790 | brk, 1.3 mm/min, 50 mm span |
Impact strength, Izod notched | 23.0 °C | 10 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 10 kJ/m² | ISO 180/1A | 80*10*4, 23°C |
Impact strength, Izod notched, ASTM | 23.0 °C | 107 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 107 J/m | ASTM D 256 |
Impact strength, Izod unnotched | 23.0 °C | 48 kJ/m² Show Supplier Material materials with Impact strength, Izod unnotched of 48 kJ/m² | ISO 180/1U | 80*10*4, 23°C |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 755 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 755 J/m | ASTM D 4812 | 23°C |
Instrumented Impact, Total Energy | 23.0 °C | 9 J Show Supplier Material materials with Instrumented Impact, Total Energy of 9 J | ASTM D 3763 | 23°C |
Tensile strength | 23.0 °C | 119 MPa Show Supplier Material materials with Tensile strength of 119 MPa | ISO 527 | break, 5 mm/min |
Thermal
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 2.7E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 2.7E-5 1/K | ASTM D 696 | -30°C to 30°C | ||
Coefficient of thermal expansion, transverse | 23.0 °C | 4.5E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion, transverse of 4.5E-5 1/K | ASTM D 696 | -30°C to 30°C | ||
Heat deflection temperature | 136 - 140 °C Show Supplier Material materials with Heat deflection temperature of 136 - 140 °C | ||||
Heat deflection temperature, 0.45 MPa | 140 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 140 °C | ISO 75/Bf | Flatw 80*10*4 sp=64mm | |||
Heat deflection temperature, 1.80 MPa | 136 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 136 °C | ISO 75/Af | Flatw 80*10*4 sp=64mm | |||
Relative temperature index, electrical | 80 °C Show Supplier Material materials with Relative temperature index, electrical of 80 °C | UL 746B | |||
Relative temperature index, mechanical impact | 80 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 80 °C | UL 746B | |||
Relative temperature index, mechanical strength | 80 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 80 °C | UL 746B | |||
Flammability | UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=101358201- - <br> UL Recognized, 94V-0 Flame Class Rating: ≥1.5mm UL 94 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 120°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |