General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 1.19 g/cm³ Show Supplier Material materials with Density of 1.19 g/cm³ | ASTM D 792 |
Relative density | 23.0 °C | 1.2 [-] Show Supplier Material materials with Relative density of 1.2 [-] | ASTM D 792 | |
Specific volume | 23.0 °C | 0.83 cm³/g Show Supplier Material materials with Specific volume of 0.83 cm³/g | ASTM D 792 |
Water absorption | 23.0 °C | 0.58 % Show Supplier Material materials with Water absorption of 0.58 % | ASTM D 570 | equilibrium, 100°C |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elongation | 23.0 °C | 135 % Show Supplier Material materials with Elongation of 135 % | ASTM D 638 | brk, Type I, 50 mm/min |
Flexural modulus | 23.0 °C | 2.3 GPa Show Supplier Material materials with Flexural modulus of 2.3 GPa | ASTM D 790 | 1.3 mm/min, 50 mm span |
Flexural strength | 23.0 °C | 97 MPa Show Supplier Material materials with Flexural strength of 97 MPa | ASTM D 790 | yld, 1.3 mm/min, 50 mm span |
Hardness, Rockwell M | 23.0 °C | 70 [-] Show Supplier Material materials with Hardness, Rockwell M of 70 [-] | ASTM D 785 | |
Hardness, Rockwell R | 23.0 °C | 118 [-] Show Supplier Material materials with Hardness, Rockwell R of 118 [-] | ASTM D 785 |
Impact strength, Izod notched | 23.0 °C | 907 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 907 kJ/m² | ASTM D 256 | notched, 23°C |
Impact strength, Izod notched, ASTM | 23.0 °C | 907 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 907 J/m | ASTM D 256 | notched, 23°C |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 3204 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 3204 J/m | ASTM D 4812 | 23°C |
Taber Abrasion | 23.0 °C | 10 mg/1000cy Show Supplier Material materials with Taber Abrasion of 10 mg/1000cy | ASTM D 1044 | CS-17, 1 kg |
Tensile strength | 23.0 °C | 68 MPa Show Supplier Material materials with Tensile strength of 68 MPa | ASTM D 638 | brk, Type I, 50 mm/min |
Thermal
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 6.84E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 6.84E-5 1/K | ASTM E 831 | -40°C to 95°C | ||
Heat deflection temperature | 132 - 137 °C Show Supplier Material materials with Heat deflection temperature of 132 - 137 °C | ||||
Heat deflection temperature, 0.45 MPa | 137 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 137 °C | ASTM D 648 | 6.4 mm, unannealed | |||
Heat deflection temperature, 1.80 MPa | 132 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 132 °C | ASTM D 648 | 6.4 mm, unannealed | |||
Relative temperature index, electrical | 130 °C Show Supplier Material materials with Relative temperature index, electrical of 130 °C | UL 746B | |||
Relative temperature index, mechanical impact | 130 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 130 °C | UL 746B | |||
Relative temperature index, mechanical strength | 130 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 130 °C | UL 746B | |||
Specific heat capacity | 23.0 °C | 1.25E-3 J/(kg·K) Show Supplier Material materials with Specific heat capacity of 1.25E-3 J/(kg·K) | ASTM C 351 | ||
Thermal conductivity | 23.0 °C | 0.29 W/(m·K) Show Supplier Material materials with Thermal conductivity of 0.29 W/(m·K) | ASTM C177 | ||
Vicat softening temperature | 154 °C Show Supplier Material materials with Vicat softening temperature of 154 °C | ASTM D 1525 | Rate B/50 | |||
Flammability | UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=103938181- - <br> UL Recognized, 94HB Flame Class Rating: ≥0.7mm UL 94 <br> UV-light, water exposure/immersion: F2- UL 746C |
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Comparative tracking index | 23.0 °C | 2 V Show Supplier Material materials with Comparative tracking index of 2 V | UL 746A | (UL) {PLC} |
Dielectric constant, 1MHz | 23.0 °C | 2.96 [-] Show Supplier Material materials with Dielectric constant, 1MHz of 2.96 [-] | ASTM D 150 |
Dielectric constant, 60Hz | 23.0 °C | 3.17 [-] Show Supplier Material materials with Dielectric constant, 60Hz of 3.17 [-] | ASTM D 150 | 50/60 Hz |
Dielectric strength | 23.0 °C | 14.9 kV/mm Show Supplier Material materials with Dielectric strength of 14.9 kV/mm | ASTM D 149 | in air, 3.2 mm |
Dissipation factor, 1MHz | 23.0 °C | 0.01 [-] Show Supplier Material materials with Dissipation factor, 1MHz of 0.01 [-] | ASTM D 150 |
Dissipation factor, 50Hz | 23.0 °C | 9E-4 [-] Show Supplier Material materials with Dissipation factor, 50Hz of 9E-4 [-] | ASTM D 150 | 50/60 Hz |
High Amp Arc Ignition | 23.0 °C | 1.1 mm Show Supplier Material materials with High Amp Arc Ignition of 1.1 mm | ≥, UL 746A | PLC 2 |
Hot-Wire Ignition | 23.0 °C | 1.1 mm Show Supplier Material materials with Hot-Wire Ignition of 1.1 mm | ≥, UL 746A | PLC 3 |
Volume resistivity | 23.0 °C | 1.00E+17 Ω·cm Show Supplier Material materials with Volume resistivity of 1.00E+17 Ω·cm | >, ASTM D 257 |
Optical
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Electronic Components | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 120°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |