General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 1.39 g/cm³ Show Supplier Material materials with Density of 1.39 g/cm³ | ISO 1183 |
Water absorption | 23.0 °C | 2.64 % Show Supplier Material materials with Water absorption of 2.64 % | ISO 62-1 | (23°C/24hrs) |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 9.4 GPa Show Supplier Material materials with Elastic modulus of 9.4 GPa | ISO 527 | 1 mm/min |
Elongation | 23.0 °C | 2.4 % Show Supplier Material materials with Elongation of 2.4 % | ISO 527 | break, 5 mm/min |
Flexural modulus | 23.0 °C | 8 GPa Show Supplier Material materials with Flexural modulus of 8 GPa | ISO 178 | 2 mm/min |
Flexural strength | 23.0 °C | 190 MPa Show Supplier Material materials with Flexural strength of 190 MPa | ISO 178 | yield, 2 mm/min |
Impact strength, Izod notched | 23.0 °C | 7 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 7 kJ/m² | ISO 180/1A | 80*10*4, 23°C |
Impact strength, Izod unnotched | 23.0 °C | 45 kJ/m² Show Supplier Material materials with Impact strength, Izod unnotched of 45 kJ/m² | ISO 180/1U | unnotched 80*10*4, 23°C |
Tensile strength | 23.0 °C | 130 MPa Show Supplier Material materials with Tensile strength of 130 MPa | ISO 527 | break, 5 mm/min |
Thermal
Property | Value | Comment | |
---|---|---|---|
Ball pressure temperature | 240 °C Show Supplier Material materials with Ball pressure temperature of 240 °C | IEC 60695-10-2 | approximate maximum | |
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | IEC 60695-2-12 | 0.4 mm | |
Glow Wire Ignition Temperature | 775 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 775 °C | IEC 60695-2-13 | 0.9 mm | |
Heat deflection temperature | 240 °C Show Supplier Material materials with Heat deflection temperature of 240 °C | ||
Heat deflection temperature, 1.80 MPa | 240 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 240 °C | ISO 75/Af | Flatw 80*10*4 sp=64mm | |
Relative temperature index, electrical | 140 °C Show Supplier Material materials with Relative temperature index, electrical of 140 °C | UL 746B | |
Relative temperature index, mechanical impact | 110 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 110 °C | UL 746B | |
Relative temperature index, mechanical strength | 140 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 140 °C | UL 746B | |
Flammability | UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=101345284- - <br> UL Yellow Card Link 2: https://iq.ul.com/ul/cert.aspx?ULID=101358203- - <br> UL Recognized, 94-5VA Flame Class Rating: ≥0.9mm UL 94 <br> UL Recognized, 94-5VB Flame Class Rating: ≥1.5mm UL 94 <br> UL Recognized, 94V-0 Flame Class Rating: ≥0.4mm UL 94 <br> UV-light, water exposure/immersion: F1- UL 746C <br> Glow Wire Ignitability Temperature, 1.5 mm: 775°C IEC 60695-2-13 <br> Glow Wire Ignitability Temperature, 1.0 mm: 775°C IEC 60695-2-13 <br> Glow Wire Flammability Index, 1.6 mm: 960°C IEC 60695-2-12 <br> Glow Wire Flammability Index, 1.5 mm: 960°C IEC 60695-2-12 <br> Glow Wire Flammability Index, 0.8 mm: 960°C IEC 60695-2-12 <br> UL Yellow Card Link 3: https://iq.ul.com/ul/cert.aspx?ULID=101345251- - <br> UL Yellow Card Link 4: https://iq.ul.com/ul/cert.aspx?ULID=102614475- - |
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Comparative tracking index | 23.0 °C | 0 V Show Supplier Material materials with Comparative tracking index of 0 V | UL 746A | (UL) {PLC} |
Dielectric strength | 23.0 °C | 16 kV/mm Show Supplier Material materials with Dielectric strength of 16 kV/mm | ASTM D 149 | in air, 1.6 mm |
High Amp Arc Ignition | 23.0 °C | 0.4 mm Show Supplier Material materials with High Amp Arc Ignition of 0.4 mm | ≥, UL 746A | PLC 0 |
High Volt Arc Track Rate | 23.0 °C | 0 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 0 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 0.4 mm Show Supplier Material materials with Hot-Wire Ignition of 0.4 mm | ≥, UL 746A | PLC 0 |
Volume resistivity | 23.0 °C | 1.00E+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1.00E+12 Ω·cm | ASTM D 257 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Displays, Building Element, Battery Pack, Circuit Protection, EV Infrastructure, Heavy Vehicles, Energy Management, Enclosures, Electronic Components, Personal Computing, Security/Detection, Wiring Devices | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 80°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |