General
Property | Temperature | Value | Comment |
---|---|---|---|
Water absorption | 23.0 °C | 3.6 % Show Supplier Material materials with Water absorption of 3.6 % | ASTM D 570 | (23°C/Saturated) |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elongation | 23.0 °C | 52 % Show Supplier Material materials with Elongation of 52 % | ASTM D 638 | brk, Type I, 50 mm/min |
Flexural modulus | 23.0 °C | 2.2 GPa Show Supplier Material materials with Flexural modulus of 2.2 GPa | ASTM D 790 | 2.6 mm/min, 100 mm span |
Flexural strength | 23.0 °C | 89 MPa Show Supplier Material materials with Flexural strength of 89 MPa | ASTM D 790 | yld, 2.6 mm/min, 100 mm span |
Impact strength, Izod notched | 23.0 °C | 272 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 272 kJ/m² | ASTM D 256 | notched, 23°C |
Taber Abrasion | 23.0 °C | 19 mg/1000cy Show Supplier Material materials with Taber Abrasion of 19 mg/1000cy | ASTM D 1044 | CS-17, 1 kg |
Tensile strength | 23.0 °C | 56 MPa Show Supplier Material materials with Tensile strength of 56 MPa | ASTM D 638 | brk, Type I, 50 mm/min |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 9.3E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 9.3E-5 1/K | ASTM E 831 | 23°C to 80°C |
Heat deflection temperature | 155 °C Show Supplier Material materials with Heat deflection temperature of 155 °C | ||
Heat deflection temperature, 0.45 MPa | 155 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 155 °C | ASTM D 648 | 6.4 mm, unannealed | |
Vicat softening temperature | 232 °C Show Supplier Material materials with Vicat softening temperature of 232 °C | ASTM D 1525 | Rate B/50 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Shrinkage | 23.0 °C | 1.2 % Show Supplier Material materials with Shrinkage of 1.2 % | SABIC method | on tensile bar |
Technological properties
Property | ||
---|---|---|
Application areas | Wheel Cover, Recreational Vehicle, Auto Aftermarket | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 95 to 105.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |