Description

NORYL™ N1050 resin is a non-reinforced blend of polyphenylene ether (PPE) + high impact polystyrene (HIPS). This injection moldable grade was designed for improved dimensional stability and flow. This grade contains non-brominated, non-chlorinated flame retardant and carries a UL94 flame rating of 5VA at 2.5mm and V0 at 1.5mm along with impact strength, very low moisture absorption, excellent dimensional stability, and good electrical properties. NORYL N1050 resin is an excellent candidate for a variety of applications requiring electrically insulating properties, low moisture absorption and low warpage.

This material data has been provided by Sabic.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyTemperatureValueComment

Relative density

23.0 °C

1.1 [-]

Show Supplier Material materials with Relative density of 1.1 [-]

ASTM D 792 |

Water absorption

23.0 °C

0.07 %

Show Supplier Material materials with Water absorption of 0.07 %

ASTM D 570 | (23°C/24hrs)

Mechanical

PropertyTemperatureValueComment

Elongation

23.0 °C

40 %

Show Supplier Material materials with Elongation of 40 %

SABIC - Japan Method | break

Flexural modulus

23.0 °C

2.5 GPa

Show Supplier Material materials with Flexural modulus of 2.5 GPa

ASTM D 790

Flexural strength

23.0 °C

98 MPa

Show Supplier Material materials with Flexural strength of 98 MPa

ASTM D 790

Impact strength, Izod notched

23.0 °C

117 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 117 kJ/m²

ASTM D 256 | notched, 23°C

Impact strength, Izod notched, ASTM

23.0 °C

117 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 117 J/m

ASTM D 256 | notched, 23°C

Tensile strength

23.0 °C

63 MPa

Show Supplier Material materials with Tensile strength of 63 MPa

SABIC - Japan Method | yield

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

7E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 7E-5 1/K

TMA | -30°C to 30°C

Heat deflection temperature

105 °C

Show Supplier Material materials with Heat deflection temperature of 105 °C

Heat deflection temperature, 1.80 MPa

105 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 105 °C

ASTM D 648 | 6.4 mm, unannealed

Flammability

UL Recognized, 94V-0 Flame Class Rating: 1.5mm UL 94 <br> UL Recognized, 94-5VA Flame Class Rating: 2.5mm UL 94

Electrical

PropertyTemperatureValueComment

Dielectric constant, 60Hz

23.0 °C

2.78 [-]

Show Supplier Material materials with Dielectric constant, 60Hz of 2.78 [-]

ASTM D 150 | 50/60 Hz

Dissipation factor, 50Hz

23.0 °C

3E-3 [-]

Show Supplier Material materials with Dissipation factor, 50Hz of 3E-3 [-]

ASTM D 150 | 50/60 Hz

Sheet resistivity, ROA

23.0 °C

1.00E+16 Ω

Show Supplier Material materials with Sheet resistivity, ROA of 1.00E+16 Ω

ASTM D 257

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

17 g/10min

Show Supplier Material materials with Melt mass-flow rate of 17 g/10min

ASTM D 1238 | 250°C/10.0 kgf

Shrinkage

23.0 °C

0.5 %

Show Supplier Material materials with Shrinkage of 0.5 %

SABIC method | 3.2 mm

Technological properties

Property
Application areas

Photovoltaic Components, Power Manangement, Personal Computing, Washing Machine, Wireless Communications, Document Handling, Displays, Battery Cell, Battery Pack, Auto Electrical, EV Infrastructure, EV/HEV Battery, Enclosures, Energy Management, Enclosure/Housing/Cover, Electronic Components

Availability

Europe,Asia,Americas

Processing methods

Drying Temperature: 75 to 80.0°C
Drying Time: 3 to 4.0hrs
Drying Time (Cumulative): 8hrs
Maximum Moisture Content: 0.02%
Melt Temperature: 250 to 275.0°C
Nozzle Temperature: 250 to 275.0°C
Front - Zone 3 Temperature: 240 to 275.0°C
Middle - Zone 2 Temperature: 225 to 270.0°C
Rear - Zone 1 Temperature: 215 to 265.0°C
Mold Temperature: 55 to 75.0°C
Back Pressure: 0.3 to 0.7MPa
Screw Speed: 20 to 100.0rpm
Shot to Cylinder Size: 30 to 70.0%
Vent Depth: 0.038 to 0.051mm

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.