General
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 5.9 GPa Show Supplier Material materials with Elastic modulus of 5.9 GPa | ASTM D 638 | 50 mm/min |
Elongation | 23.0 °C | 2 % Show Supplier Material materials with Elongation of 2 % | ASTM D 638 | brk, Type I, 5 mm/min |
Flexural modulus | 23.0 °C | 5.4 GPa Show Supplier Material materials with Flexural modulus of 5.4 GPa | ASTM D 790 | 1.3 mm/min, 50 mm span |
Flexural strength | 23.0 °C | 96 MPa Show Supplier Material materials with Flexural strength of 96 MPa | ASTM D 790 | brk, 1.3 mm/min, 50 mm span |
Impact strength, Izod notched | 23.0 °C | 42 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 42 kJ/m² | ASTM D 256 | notched, 23°C |
Impact strength, Izod notched, ASTM | 23.0 °C | 42 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 42 J/m | ASTM D 256 | notched, 23°C |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 240 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 240 J/m | ASTM D 4812 | 23°C |
Tensile strength | 23.0 °C | 62 MPa Show Supplier Material materials with Tensile strength of 62 MPa | ASTM D 638 | yld, Type I, 5 mm/min |
Thermal
Property | Value | Comment | |
---|---|---|---|
Heat deflection temperature | 96 °C Show Supplier Material materials with Heat deflection temperature of 96 °C | ||
Heat deflection temperature, 1.80 MPa | 96 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 96 °C | ASTM D 648 | 3.2mm, unannealed | |
Relative temperature index, electrical | 60 °C Show Supplier Material materials with Relative temperature index, electrical of 60 °C | UL 746B | |
Relative temperature index, mechanical impact | 60 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 60 °C | UL 746B | |
Relative temperature index, mechanical strength | 60 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 60 °C | UL 746B | |
Flammability | UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=101345220- - <br> UL Recognized, 94HB Flame Class Rating: ≥1.5mm UL 94 |
Electrical
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Electronic Components, Wireless Communications, Wiring Devices | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 80°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |