LNP™ STAT-KON™ Compound Noryl_HMC1010

Want to keep this datasheet? Save it now in your required format

Description

LNP™ STAT-KON™ Noryl_HMC1010 compound is a 10% Carbon fiber reinforced. Static dissipative. Nonbrominated, nonchlor- nated flame retardant system. UL94 V-1 rated.

This material data has been provided by Sabic.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyTemperatureValueComment

Relative density

23.0 °C

1.15 [-]

Show Supplier Material materials with Relative density of 1.15 [-]

ASTM D 792

Mechanical

PropertyTemperatureValueComment

Elongation

23.0 °C

3 %

Show Supplier Material materials with Elongation of 3 %

ASTM D 638 | brk, Type I, 5 mm/min

Flexural modulus

23.0 °C

6.9 GPa

Show Supplier Material materials with Flexural modulus of 6.9 GPa

ASTM D 790 | 2.6 mm/min, 100 mm span

Flexural strength

23.0 °C

103 MPa

Show Supplier Material materials with Flexural strength of 103 MPa

ASTM D 790 | yld, 2.6 mm/min, 100 mm span

Hardness, Rockwell R

23.0 °C

122 [-]

Show Supplier Material materials with Hardness, Rockwell R of 122 [-]

ASTM D 785

Impact strength, Izod notched

23.0 °C

69 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 69 kJ/m²

ASTM D 256 | notched, 23°C

Impact strength, Izod notched, ASTM

23.0 °C

69 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 69 J/m

ASTM D 256 | notched, 23°C

Impact strength, Izod unnotched, ASTM

23.0 °C

240 J/m

Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 240 J/m

ASTM D 4812 | 23°C

Taber Abrasion

23.0 °C

83 mg/1000cy

Show Supplier Material materials with Taber Abrasion of 83 mg/1000cy

ASTM D 1044 | CS-17, 1 kg

Tensile strength

23.0 °C

71 MPa

Show Supplier Material materials with Tensile strength of 71 MPa

ASTM D 638 | brk, Type I, 5 mm/min

Thermal

PropertyValueComment

Heat deflection temperature

105 - 111 °C

Show Supplier Material materials with Heat deflection temperature of 105 - 111 °C

Heat deflection temperature, 0.45 MPa

111 °C

Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 111 °C

ASTM D 648 | 6.4 mm, unannealed

Heat deflection temperature, 1.80 MPa

105 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 105 °C

ASTM D 648 | 6.4 mm, unannealed

Flammability

UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=221166- - <br> UL Recognized, 94V-1 Flame Class Rating: 2mm UL 94 <br> UL Recognized, 94-5VA Flame Class Rating: 2mm UL 94

Electrical

PropertyTemperatureValueComment

Sheet resistivity, ROA

23.0 °C

13000 Ω

Show Supplier Material materials with Sheet resistivity, ROA of 13000 Ω

ASTM D 257

Volume resistivity

23.0 °C

8000 Ω·cm

Show Supplier Material materials with Volume resistivity of 8000 Ω·cm

ASTM D 257

Rheological Properties

PropertyTemperatureValueComment

Shrinkage

23.0 °C

0.05 %

Show Supplier Material materials with Shrinkage of 0.05 %

SABIC method | 3.2 mm

Shrinkage, transverse

23.0 °C

0.15 %

Show Supplier Material materials with Shrinkage, transverse of 0.15 %

SABIC method | 3.2 mm

Technological properties

Property
Application areas

Electrical Components & Infrastructure

Availability

Europe,Asia,Americas

Processing methods

Drying Temperature: 90 to 95.0°C
Drying Time: 3 to 4.0hrs
Drying Time (Cumulative): 8hrs
Maximum Moisture Content: 0.02%
Melt Temperature: 255 to 280.0°C
Nozzle Temperature: 255 to 280.0°C
Front - Zone 3 Temperature: 245 to 280.0°C
Middle - Zone 2 Temperature: 230 to 275.0°C
Rear - Zone 1 Temperature: 220 to 270.0°C
Mold Temperature: 65 to 90.0°C
Back Pressure: 0.3 to 0.7MPa
Screw Speed: 20 to 100.0rpm
Shot to Cylinder Size: 30 to 70.0%
Vent Depth: 0.038 to 0.051mm

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.