General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 1.45 g/cm³ Show Supplier Material materials with Density of 1.45 g/cm³ | ISO 1183 |
Moisture absorption | 23.0 °C | 0.2 % Show Supplier Material materials with Moisture absorption of 0.2 % | ASTM D 570 | (23°C/50% RH/24 hrs) |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 11.3 GPa Show Supplier Material materials with Elastic modulus of 11.3 GPa | ISO 527 | 1 mm/min |
Elongation | 23.0 °C | 1.9 % Show Supplier Material materials with Elongation of 1.9 % | ISO 527 | break, 5 mm/min |
Flexural modulus | 23.0 °C | 9.1 GPa Show Supplier Material materials with Flexural modulus of 9.1 GPa | ISO 178 | 2 mm/min |
Flexural strength | 23.0 °C | 189 MPa Show Supplier Material materials with Flexural strength of 189 MPa | ISO 178 |
Impact strength, Izod notched | 23.0 °C | 5 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 5 kJ/m² | ISO 180/1A | notched 80*10*4, 23°C |
Impact strength, Izod notched, ASTM | 23.0 °C | 64 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 64 J/m | ASTM D 256 | notched, 23°C |
Impact strength, Izod unnotched | 23.0 °C | 32 kJ/m² Show Supplier Material materials with Impact strength, Izod unnotched of 32 kJ/m² | ISO 180/1U | unnotched 80*10*4, 23°C |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 662 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 662 J/m | ASTM D 4812 | 23°C |
Tensile strength | 23.0 °C | 128 MPa Show Supplier Material materials with Tensile strength of 128 MPa | ISO 527 | break, 5 mm/min |
Thermal
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 2.5E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 2.5E-5 1/K | ISO 11359-2 | -40°C to 40°C | ||
Coefficient of thermal expansion, transverse | 23.0 °C | 5.11E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion, transverse of 5.11E-5 1/K | ISO 11359-2 | -40°C to 40°C | ||
Heat deflection temperature | 277 - 299 °C Show Supplier Material materials with Heat deflection temperature of 277 - 299 °C | ||||
Heat deflection temperature, 0.45 MPa | 299 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 299 °C | ASTM D 648 | 3.2 mm, unannealed | |||
Heat deflection temperature, 1.80 MPa | 277 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 277 °C | ISO 75/Af | Flatw 80*10*4 sp=64mm | |||
Relative temperature index, electrical | 125 °C Show Supplier Material materials with Relative temperature index, electrical of 125 °C | UL 746B | |||
Relative temperature index, mechanical impact | 50 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 50 °C | UL 746B | |||
Relative temperature index, mechanical strength | 125 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 125 °C | UL 746B | |||
Flammability | UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=101284114- - <br> UL Yellow Card Link 2: https://iq.ul.com/ul/cert.aspx?ULID=103093678- - <br> UL Recognized, 94V-0 Flame Class Rating: ≥1.5mm UL 94 <br> UL Recognized, 94V-1 Flame Class Rating: ≥1mm UL 94 |
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Comparative tracking index | 23.0 °C | 0 V Show Supplier Material materials with Comparative tracking index of 0 V | UL 746A | (UL) {PLC} |
Dielectric constant, 1MHz | 23.0 °C | 3.82 [-] Show Supplier Material materials with Dielectric constant, 1MHz of 3.82 [-] | ASTM D 150 |
Dielectric strength | 23.0 °C | 29.7 kV/mm Show Supplier Material materials with Dielectric strength of 29.7 kV/mm | ASTM D 149 | in oil, 0.8 mm |
Dissipation factor, 1MHz | 23.0 °C | 0.01 [-] Show Supplier Material materials with Dissipation factor, 1MHz of 0.01 [-] | ASTM D 150 | |
Dissipation factor, 1kHz | 23.0 °C | 0.01 [-] Show Supplier Material materials with Dissipation factor, 1kHz of 0.01 [-] | ASTM D 150 |
High Volt Arc Track Rate | 23.0 °C | 2 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 2 PLC Code | UL 746A | (PLC) |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Electronic Components, Data Transfer | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 90 to 110.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |