Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 8.3 GPa Show Supplier Material materials with Elastic modulus of 8.3 GPa | ASTM D 638 | 50 mm/min |
Elongation | 23.0 °C | 2.7 % Show Supplier Material materials with Elongation of 2.7 % | ASTM D 638 | break |
Flexural modulus | 23.0 °C | 7.6 GPa Show Supplier Material materials with Flexural modulus of 7.6 GPa | ASTM D 790 |
Flexural strength | 23.0 °C | 179 MPa Show Supplier Material materials with Flexural strength of 179 MPa | ASTM D 790 |
Impact strength, Izod notched | 23.0 °C | 64 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 64 kJ/m² | ASTM D 256 | notched, 23°C |
Impact strength, Izod notched, ASTM | 23.0 °C | 64 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 64 J/m | ASTM D 256 | notched, 23°C |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 534 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 534 J/m | ASTM D 4812 | 23°C |
Tensile strength | 23.0 °C | 110 MPa Show Supplier Material materials with Tensile strength of 110 MPa | ASTM D 638 | break |
Thermal
Property | Value | Comment | |
---|---|---|---|
Heat deflection temperature | 141 °C Show Supplier Material materials with Heat deflection temperature of 141 °C | ||
Heat deflection temperature, 1.80 MPa | 141 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 141 °C | ASTM D 648 | 3.2mm, unannealed | |
Relative temperature index, electrical | 80 °C Show Supplier Material materials with Relative temperature index, electrical of 80 °C | UL 746B | |
Relative temperature index, mechanical impact | 80 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 80 °C | UL 746B | |
Relative temperature index, mechanical strength | 80 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 80 °C | UL 746B | |
Flammability | UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=101345261- - <br> UL Recognized, 94-5VA Flame Class Rating: ≥3mm UL 94 <br> UL Recognized, 94V-0 Flame Class Rating: ≥1.5mm UL 94 |
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Sheet resistivity, ROA | 23.0 °C | 10 - 1000000 Ω Show Supplier Material materials with Sheet resistivity, ROA of 10 - 1000000 Ω | ASTM D 257 |
Technological properties
Property | ||
---|---|---|
Application areas | ATM/Ticket Machine | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 120°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |