LEXAN™ Copolymer DMX1435 - Asia

Want to keep this datasheet? Save it now in your required format

Description

LEXAN™ DMX1435 is a UV stabilized standard flow polycarbonate copolymer resin with improved scratch resistance, improved dielectric performance (lower Df). It is both transparency and colorable available solutions to the applications such as 5G related devices, anti-scratch covers, etc.

This material data has been provided by Sabic.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.17 g/cm³

Show Supplier Material materials with Density of 1.17 g/cm³

ISO 1183

Moisture absorption

23.0 °C

0.13 %

Show Supplier Material materials with Moisture absorption of 0.13 %

ISO 62 | (23°C / 50% RH)

Relative density

23.0 °C

1.2 [-]

Show Supplier Material materials with Relative density of 1.2 [-]

ASTM D 792 |

Specific volume

23.0 °C

0.85 cm³/g

Show Supplier Material materials with Specific volume of 0.85 cm³/g

ASTM D 792

Water absorption

23.0 °C

0.27 %

Show Supplier Material materials with Water absorption of 0.27 %

ISO 62-1 | (23°C/saturated)

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

2.5 GPa

Show Supplier Material materials with Elastic modulus of 2.5 GPa

ISO 527 | 1 mm/min

Elongation

23.0 °C

7 %

Show Supplier Material materials with Elongation of 7 %

ISO 527 | yield, 50 mm/min

Erichson scratch depth

23.0 °C

14 µm

Show Supplier Material materials with Erichson scratch depth of 14 µm

SABIC method | 6N

Flexural modulus

23.0 °C

2.5 GPa

Show Supplier Material materials with Flexural modulus of 2.5 GPa

ISO 178 | 2 mm/min

Flexural strength

23.0 °C

108 MPa

Show Supplier Material materials with Flexural strength of 108 MPa

ISO 178 | yield, 2 mm/min

Hardness, Ball Indentation

23.0 °C

128 MPa

Show Supplier Material materials with Hardness, Ball Indentation of 128 MPa

ISO 2039-1 | H358/30

Hardness, Pencil test

H

ASTM D 3363 | 1kgf

Hardness, Rockwell L

23.0 °C

108 [-]

Show Supplier Material materials with Hardness, Rockwell L of 108 [-]

ASTM D 785

Hardness, Rockwell M

23.0 °C

93 [-]

Show Supplier Material materials with Hardness, Rockwell M of 93 [-]

ASTM D 785 |

Impact strength, Charpy notched

23.0 °C

3 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 3 kJ/m²

ISO 179/1eA | V-notch Edgew 80*10*3 sp=62mm, 23°C

Impact strength, Izod notched

23.0 °C

5 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 5 kJ/m²

ISO 180/1A | 80*10*3, 23°C

Impact strength, Izod notched, ASTM

23.0 °C

30 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 30 J/m

ASTM D 256 | notched, 23°C

Instrumented Impact, Total Energy

23.0 °C

30 J

Show Supplier Material materials with Instrumented Impact, Total Energy of 30 J

ASTM D 3763 | 23°C

Taber Abrasion

23.0 °C

10 mg/1000cy

Show Supplier Material materials with Taber Abrasion of 10 mg/1000cy

SABIC method | CS-17, 1 kg

Tensile strength

23.0 °C

60 MPa

Show Supplier Material materials with Tensile strength of 60 MPa

ISO 527 | break, 50 mm/min

Impact strength, Charpy unnotched

ISO 179/1eU | Unnotch Edgew 80*10*3 sp=62mm, 23°C

Impact strength, Izod unnotched

ISO 180/1U | 80*10*3, -30°C

Impact strength, Izod unnotched, ASTM

ASTM D 4812 | 23°C

Thermal

PropertyTemperatureValueComment

Ball Pressure Test

nan

IEC 60695-10-2 | 125°C +/- 2°C

Ball pressure temperature

140 °C

Show Supplier Material materials with Ball pressure temperature of 140 °C

IEC 60695-10-2 | approximate maximum

Coefficient of thermal expansion

23.0 °C

7E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 7E-5 1/K

ISO 11359-2 | 23°C to 80°C

Coefficient of thermal expansion, transverse

23.0 °C

7E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion, transverse of 7E-5 1/K

ISO 11359-2 | 23°C to 80°C

Glow Wire Flammability Index

960 °C

Show Supplier Material materials with Glow Wire Flammability Index of 960 °C

Glow Wire Ignition Temperature

825 °C

Show Supplier Material materials with Glow Wire Ignition Temperature of 825 °C

IEC 60695-2-13 | 2.0 mm

Heat deflection temperature

118 - 131 °C

Show Supplier Material materials with Heat deflection temperature of 118 - 131 °C

Heat deflection temperature, 0.45 MPa

131 °C

Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 131 °C

ISO 75/Bf | Flatw 80*10*4 sp=64mm

Heat deflection temperature, 1.80 MPa

118 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 118 °C

ISO 75/Af | Flatw 80*10*4 sp=64mm

Relative temperature index, electrical

80 °C

Show Supplier Material materials with Relative temperature index, electrical of 80 °C

UL 746B

Relative temperature index, mechanical impact

80 °C

Show Supplier Material materials with Relative temperature index, mechanical impact of 80 °C

UL 746B

Relative temperature index, mechanical strength

80 °C

Show Supplier Material materials with Relative temperature index, mechanical strength of 80 °C

UL 746B

Specific heat capacity

23.0 °C

1.4E-3 J/(kg·K)

Show Supplier Material materials with Specific heat capacity of 1.4E-3 J/(kg·K)

ASTM C 351

Thermal conductivity

23.0 °C

0.2 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 0.2 W/(m·K)

ISO 8302

Vicat softening temperature

138 °C

Show Supplier Material materials with Vicat softening temperature of 138 °C

ISO 306 | Rate B/50

Flammability

UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=100081387- - <br> UL Recognized, 94HB Flame Class Rating: ≥0.6mm UL 94 <br> Glow Wire Ignitability Temperature, 1.0 mm: 850°C IEC 60695-2-13 <br> Glow Wire Flammability Index, 1.0 mm: 900°C IEC 60695-2-12

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

2 V

Show Supplier Material materials with Comparative tracking index of 2 V

UL 746A | (UL) {PLC}

Optical

PropertyValueComment

Haze

0.8 %

Show Supplier Material materials with Haze of 0.8 %

<, ASTM D 1003 | 2.54 mm

Refractive index

1.58 [-]

Show Supplier Material materials with Refractive index of 1.58 [-]

ISO 489

Transmission

88 %

Show Supplier Material materials with Transmission of 88 %

ASTM D 1003 | 2.54 mm

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

14.5 g/10min

Show Supplier Material materials with Melt mass-flow rate of 14.5 g/10min

ASTM D 1238 | 300°C/1.2 kgf

Melt volume-flow rate

13 cm³/10min

Show Supplier Material materials with Melt volume-flow rate of 13 cm³/10min

ISO 1133 | MVR at 300°C/1.2 kg

Shrinkage

23.0 °C

0.5 %

Show Supplier Material materials with Shrinkage of 0.5 %

SABIC method | 3.2 mm

Technological properties

Property
Application areas

Medical Device, Motorcycle, Non-LED Lighting, Personal Computing, Wiring Devices, Wireless Communications, Cluster, City, Auto Aftermarket, Audio, Building Accessory, Air Conditioning, Fluid Delivery, Enclosures, Electronic Components

Availability

Asia

Processing methods

Drying Temperature: 120°C
Drying Time: 3 to 4.0hrs
Maximum Moisture Content: 0.02%
Melt Temperature: 295 to 315.0°C
Nozzle Temperature: 290 to 310.0°C
Front - Zone 3 Temperature: 295 to 315.0°C
Middle - Zone 2 Temperature: 280 to 305.0°C
Rear - Zone 1 Temperature: 260 to 280.0°C
Hopper Temperature: 60 to 80.0°C
Mold Temperature: 70 to 95.0°C

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.