Description

LNP™ THEMROTUF™ PF003IU is a Polyamide 6 compound,17% glass filled, fiber reinforced, with impact modifier and UV stabilized.

This material data has been provided by Sabic.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

Mechanical

PropertyTemperatureValueComment

Flexural modulus

23.0 °C

4.1 GPa

Show Supplier Material materials with Flexural modulus of 4.1 GPa

ASTM D 790 | 1.3 mm/min, 50 mm span

Flexural strength

23.0 °C

145 MPa

Show Supplier Material materials with Flexural strength of 145 MPa

ASTM D 790 | yld, 1.3 mm/min, 50 mm span

Impact strength, Izod notched

23.0 °C

65 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 65 kJ/m²

ASTM D 256 | notched, 23°C

Impact strength, Izod notched, ASTM

23.0 °C

65 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 65 J/m

ASTM D 256

Impact strength, Izod unnotched, ASTM

23.0 °C

610 J/m

Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 610 J/m

ASTM D 4812 | 23°C

Tensile strength

23.0 °C

103 MPa

Show Supplier Material materials with Tensile strength of 103 MPa

ASTM D 638 | brk, Type I, 50 mm/min

Thermal

PropertyValueComment

Heat deflection temperature

197 - 215 °C

Show Supplier Material materials with Heat deflection temperature of 197 - 215 °C

Heat deflection temperature, 0.45 MPa

215 °C

Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 215 °C

ASTM D 648 | 3.2 mm, unannealed

Heat deflection temperature, 1.80 MPa

197 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 197 °C

ASTM D 648 | 3.2mm, unannealed

Vicat softening temperature

201 °C

Show Supplier Material materials with Vicat softening temperature of 201 °C

ASTM D 1525 | Rate B/50

Technological properties

Property
Application areas

Enclosures

Availability

Europe,Asia,Americas

Processing methods

Drying Temperature: 100 to 110.0°C
Drying Time: 3hrs
Maximum Moisture Content: 0.02%
Melt Temperature: 250 to 265.0°C
Nozzle Temperature: 245 to 260.0°C
Front - Zone 3 Temperature: 250 to 265.0°C
Middle - Zone 2 Temperature: 245 to 260.0°C
Rear - Zone 1 Temperature: 240 to 255.0°C
Mold Temperature: 65 to 90.0°C
Screw Speed: 50 to 80.0rpm
Back Pressure: 0.3 to 0.7MPa

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.