LNP™ THERMOCOMP™ Compound MF004AS

Want to keep this datasheet? Save it now in your required format

Description

LNP THERMOCOMP* MF004AS is a compound based on Polypropylene resin containing 20% Glass Fiber. Added features of this material include: Heat Stabilized.

This material data has been provided by Sabic.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.03 g/cm³

Show Supplier Material materials with Density of 1.03 g/cm³

ISO 1183

Moisture absorption

23.0 °C

0.03 %

Show Supplier Material materials with Moisture absorption of 0.03 %

ASTM D 570 | (23°C/50% RH/24 hrs)

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

5.1 GPa

Show Supplier Material materials with Elastic modulus of 5.1 GPa

ISO 527 | 1 mm/min

Elongation

23.0 °C

2.2 %

Show Supplier Material materials with Elongation of 2.2 %

ISO 527 | break

Flexural modulus

23.0 °C

5.6 GPa

Show Supplier Material materials with Flexural modulus of 5.6 GPa

ISO 178

Flexural strength

23.0 °C

104 MPa

Show Supplier Material materials with Flexural strength of 104 MPa

ISO 178

Impact strength, Izod notched

23.0 °C

5 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 5 kJ/m²

ISO 180/1A | 80*10*4, 23°C

Impact strength, Izod notched, ASTM

23.0 °C

48 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 48 J/m

ASTM D 256 | notched, 23°C

Impact strength, Izod unnotched

23.0 °C

20 kJ/m²

Show Supplier Material materials with Impact strength, Izod unnotched of 20 kJ/m²

ISO 180/1U | 80*10*4, 23°C

Impact strength, Izod unnotched, ASTM

23.0 °C

325 J/m

Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 325 J/m

ASTM D 4812 | 23°C

Instrumented Impact, at Peak

23.0 °C

8 J

Show Supplier Material materials with Instrumented Impact, at Peak of 8 J

ASTM D 3763 | 23°C

Tensile strength

23.0 °C

65 MPa

Show Supplier Material materials with Tensile strength of 65 MPa

ISO 527 | break

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion, transverse

23.0 °C

7.45E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion, transverse of 7.45E-5 1/K

ISO 11359-2 | -40°C to 40°C

Heat deflection temperature

145 - 160 °C

Show Supplier Material materials with Heat deflection temperature of 145 - 160 °C

Heat deflection temperature, 0.45 MPa

160 °C

Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 160 °C

ASTM D 648 | 3.2 mm, unannealed

Heat deflection temperature, 1.80 MPa

145 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 145 °C

ISO 75/Af | Flatw 80*10*4 sp=64mm

Relative temperature index, electrical

105 °C

Show Supplier Material materials with Relative temperature index, electrical of 105 °C

UL 746B

Relative temperature index, mechanical impact

105 °C

Show Supplier Material materials with Relative temperature index, mechanical impact of 105 °C

UL 746B

Relative temperature index, mechanical strength

105 °C

Show Supplier Material materials with Relative temperature index, mechanical strength of 105 °C

UL 746B

Flammability

UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=101284109- - <br> UL Recognized, 94HB Flame Class Rating: ≥0.75mm UL 94

Electrical

PropertyTemperatureValueComment

High Amp Arc Ignition

23.0 °C

0.75 mm

Show Supplier Material materials with High Amp Arc Ignition of 0.75 mm

≥, UL 746A | PLC 0

High Volt Arc Track Rate

23.0 °C

0 PLC Code

Show Supplier Material materials with High Volt Arc Track Rate of 0 PLC Code

UL 746A | (PLC)

Hot-Wire Ignition

23.0 °C

0.75 mm

Show Supplier Material materials with Hot-Wire Ignition of 0.75 mm

≥, UL 746A | PLC 4

Rheological Properties

PropertyTemperatureValueComment

Shrinkage

23.0 °C

0.72 %

Show Supplier Material materials with Shrinkage of 0.72 %

ISO 294 | 24 hrs

Shrinkage, transverse

23.0 °C

0.95 %

Show Supplier Material materials with Shrinkage, transverse of 0.95 %

ISO 294 | 24 hrs

Technological properties

Property
Application areas

Pharmaceutical Manufacturing

Availability

Europe,Asia,Americas

Processing methods

Drying Temperature: 80°C
Drying Time: 4hrs
Melt Temperature: 225 to 250.0°C
Front - Zone 3 Temperature: 240 to 250.0°C
Middle - Zone 2 Temperature: 215 to 225.0°C
Rear - Zone 1 Temperature: 195 to 205.0°C
Mold Temperature: 30 to 50.0°C
Back Pressure: 0.2 to 0.3MPa
Screw Speed: 30 to 60.0rpm

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.