General
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 35.3 GPa Show Supplier Material materials with Elastic modulus of 35.3 GPa | ISO 527 | 1 mm/min |
Elongation | 23.0 °C | 1.5 % Show Supplier Material materials with Elongation of 1.5 % | ISO 527 | break, 5 mm/min |
Flexural modulus | 23.0 °C | 27.2 GPa Show Supplier Material materials with Flexural modulus of 27.2 GPa | ISO 178 | 2 mm/min |
Flexural strength | 23.0 °C | 457 MPa Show Supplier Material materials with Flexural strength of 457 MPa | ISO 178 |
Impact strength, Izod notched | 23.0 °C | 75 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 75 kJ/m² | ASTM D 256 | notched, 23°C |
Impact strength, Izod notched, ASTM | 23.0 °C | 75 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 75 J/m | ASTM D 256 | notched, 23°C |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 936 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 936 J/m | ASTM D 4812 | 23°C |
Instrumented Impact, Total Energy | 23.0 °C | 6 J Show Supplier Material materials with Instrumented Impact, Total Energy of 6 J | ASTM D 3763 | 23°C |
Poisson's ratio | 23.0 °C | 0.4 [-] Show Supplier Material materials with Poisson's ratio of 0.4 [-] | ASTM E 132 |
Shear modulus | 23.0 °C | 4.8 GPa Show Supplier Material materials with Shear modulus of 4.8 GPa | ASTM D732 |
Shear strength | 23.0 °C | 119 MPa Show Supplier Material materials with Shear strength of 119 MPa | ASTM D732 |
Tensile strength | 23.0 °C | 319 MPa Show Supplier Material materials with Tensile strength of 319 MPa | ISO 527 | break, 5 mm/min |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 5E-6 1/K Show Supplier Material materials with Coefficient of thermal expansion of 5E-6 1/K | ASTM E 831 | -40°C to 150°C |
Coefficient of thermal expansion, transverse | 23.0 °C | 3E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion, transverse of 3E-5 1/K | ASTM E 831 | -40°C to 150°C |
Heat deflection temperature | 332 °C Show Supplier Material materials with Heat deflection temperature of 332 °C | ||
Heat deflection temperature, 1.80 MPa | 332 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 332 °C | ASTM D 648 | 3.2mm, unannealed |
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Sheet resistivity, ROA | 23.0 °C | 1000 - 10000 Ω Show Supplier Material materials with Sheet resistivity, ROA of 1000 - 10000 Ω | ASTM D 257 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 150°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |