General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 1.11 g/cm³ Show Supplier Material materials with Density of 1.11 g/cm³ | ISO 1183 |
Limiting oxygen index | 23.0 °C | 30 % Show Supplier Material materials with Limiting oxygen index of 30 % | |
Relative density | 23.0 °C | 1.11 [-] Show Supplier Material materials with Relative density of 1.11 [-] | ASTM D 792 | |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 2.2 GPa Show Supplier Material materials with Elastic modulus of 2.2 GPa | ISO 527 | 1 mm/min |
Elongation | 23.0 °C | 3 % Show Supplier Material materials with Elongation of 3 % | ISO 527 | yield, 50 mm/min |
Flexural modulus | 23.0 °C | 2.2 GPa Show Supplier Material materials with Flexural modulus of 2.2 GPa | ISO 178 | 2 mm/min |
Flexural strength | 23.0 °C | 71 MPa Show Supplier Material materials with Flexural strength of 71 MPa | ISO 178 | yield, 2 mm/min |
Impact strength, Charpy notched | 23.0 °C | 5 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 5 kJ/m² | ISO 179/1eA | V-notch Edgew, 23°C, 80*10*4 sp=62mm |
Impact strength, Izod notched | 23.0 °C | 3 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 3 kJ/m² | ISO 180/1A | 80*10*4, -30°C |
Impact strength, Izod notched, ASTM | 23.0 °C | 38 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 38 J/m | ASTM D 256 |
Tensile strength | 23.0 °C | 46 MPa Show Supplier Material materials with Tensile strength of 46 MPa | ISO 527 | yield, 50 mm/min |
Thermal
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 7.7E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 7.7E-5 1/K | ISO 11359-2 | -40°C to 40°C | ||
Coefficient of thermal expansion, transverse | 23.0 °C | 7.9E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion, transverse of 7.9E-5 1/K | ISO 11359-2 | -40°C to 40°C | ||
Heat deflection temperature | 77 - 93 °C Show Supplier Material materials with Heat deflection temperature of 77 - 93 °C | ||||
Heat deflection temperature, 0.45 MPa | 93 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 93 °C | ASTM D 648 | 3.2 mm, unannealed | |||
Heat deflection temperature, 1.80 MPa | 77 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 77 °C | ISO 75/Af | Flatw 80*10*4 sp=64mm | |||
Relative temperature index, electrical | 65 °C Show Supplier Material materials with Relative temperature index, electrical of 65 °C | UL 746B | |||
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | UL 746B | |||
Relative temperature index, mechanical strength | 65 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C | UL 746B | |||
Vicat softening temperature | 101 °C Show Supplier Material materials with Vicat softening temperature of 101 °C | ISO 306 | Rate B/120 | |||
Flammability | UL Recognized, 94V-1 Flame Class Rating: 1.5mm UL 94 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=101313034- - |
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Dielectric constant, 1MHz | 23.0 °C | 2.7 [-] Show Supplier Material materials with Dielectric constant, 1MHz of 2.7 [-] | IEC 60250 |
Dissipation factor, 1MHz | 23.0 °C | 2.9E-3 [-] Show Supplier Material materials with Dissipation factor, 1MHz of 2.9E-3 [-] | IEC 60250 |
Rheological Properties
Property | Value | Comment |
---|---|---|
Melt volume-flow rate | 17 cm³/10min Show Supplier Material materials with Melt volume-flow rate of 17 cm³/10min | ISO 1133 | MVR at 280°C/1.2 kg |
Technological properties
Property | ||
---|---|---|
Availability | Europe | |
Processing methods | Nozzle Temperature: 250 to 280.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |