General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 1.51 g/cm³ Show Supplier Material materials with Density of 1.51 g/cm³ | ISO 1183 |
Moisture absorption | 23.0 °C | 0.5 % Show Supplier Material materials with Moisture absorption of 0.5 % | ISO 62 | (23°C / 50% RH) |
Relative density | 23.0 °C | 1.51 [-] Show Supplier Material materials with Relative density of 1.51 [-] | ASTM D 792 |
Water absorption | 23.0 °C | 0.9 % Show Supplier Material materials with Water absorption of 0.9 % | ISO 62-1 | (23°C/saturated) |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 9.5 GPa Show Supplier Material materials with Elastic modulus of 9.5 GPa | ISO 527 | 1 mm/min |
Elongation | 23.0 °C | 2 % Show Supplier Material materials with Elongation of 2 % | ISO 527 | yield, 5 mm/min |
Flexural modulus | 23.0 °C | 8.5 GPa Show Supplier Material materials with Flexural modulus of 8.5 GPa | ISO 178 | 2 mm/min |
Flexural strength | 23.0 °C | 225 MPa Show Supplier Material materials with Flexural strength of 225 MPa | ISO 178 | yield, 2 mm/min |
Impact strength, Charpy notched | 23.0 °C | 10 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 10 kJ/m² | ISO 179/1eA | V-notch Edgew, 23°C, 80*10*4 sp=62mm |
Impact strength, Izod notched | 23.0 °C | 10 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 10 kJ/m² | ISO 180/1A | 80*10*4, 23°C |
Impact strength, Izod notched, ASTM | 23.0 °C | 85 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 85 J/m | ASTM D 256 |
Instrumented Impact, Total Energy | 23.0 °C | 10 J Show Supplier Material materials with Instrumented Impact, Total Energy of 10 J | ASTM D 3763 | 23°C |
Tensile strength | 23.0 °C | 165 MPa Show Supplier Material materials with Tensile strength of 165 MPa | ISO 527 | break, 5 mm/min |
Thermal
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coefficient of thermal expansion | 23.0 °C | 1.6E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.6E-5 1/K | ISO 11359-2 | 23°C to 150°C | ||
Coefficient of thermal expansion, transverse | 23.0 °C | 4.1E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion, transverse of 4.1E-5 1/K | ISO 11359-2 | 23°C to 150°C | ||
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | ||||
Glow Wire Ignition Temperature | 900 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 900 °C | IEC 60695-2-13 | 2.0 mm | |||
Heat deflection temperature | 210 °C Show Supplier Material materials with Heat deflection temperature of 210 °C | ||||
Heat deflection temperature, 1.80 MPa | 210 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 210 °C | ISO 75/Af | Flatw 80*10*4 sp=64mm | |||
Relative temperature index, electrical | 180 °C Show Supplier Material materials with Relative temperature index, electrical of 180 °C | UL 746B | |||
Relative temperature index, mechanical impact | 170 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 170 °C | UL 746B | |||
Relative temperature index, mechanical strength | 180 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 180 °C | UL 746B | |||
Vicat softening temperature | 220 °C Show Supplier Material materials with Vicat softening temperature of 220 °C | ISO 306 | Rate B/120 | |||
Flammability | UL Recognized, 94-5VA Flame Class Rating: ≥1.2mm UL 94 <br> UL Recognized, 94V-0 Flame Class Rating: ≥0.25mm UL 94 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=221099- - |
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Comparative tracking index | 23.0 °C | 4 V Show Supplier Material materials with Comparative tracking index of 4 V | UL 746A | (UL) {PLC} |
High Amp Arc Ignition | 23.0 °C | 1.5 mm Show Supplier Material materials with High Amp Arc Ignition of 1.5 mm | ≥, UL 746A | PLC 3 |
High Volt Arc Track Rate | 23.0 °C | 3 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 3 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 3 mm Show Supplier Material materials with Hot-Wire Ignition of 3 mm | ≥, UL 746A | PLC 1 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Melt mass-flow rate | 7.6 g/10min Show Supplier Material materials with Melt mass-flow rate of 7.6 g/10min | ASTM D 1238 | 337°C/6.6 kgf | |
Melt volume-flow rate | 8 cm³/10min Show Supplier Material materials with Melt volume-flow rate of 8 cm³/10min | ISO 1133 | MVR at 360°C/5.0 kg | |
Shrinkage | 23.0 °C | 0.2 % Show Supplier Material materials with Shrinkage of 0.2 % | SABIC method | 3.2 mm |
Technological properties
Property | ||
---|---|---|
Application areas | Surgical Devices, Pharmaceutical Manufacturing, Medical Device, Electronic Components | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Time: 4 to 6.0hrs | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |