General
Property | Temperature | Value | Comment |
---|---|---|---|
Relative density | 23.0 °C | 1.48 [-] Show Supplier Material materials with Relative density of 1.48 [-] | ASTM D 792 |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elongation | 23.0 °C | 3 % Show Supplier Material materials with Elongation of 3 % | ASTM D 638 | brk, Type I, 5 mm/min |
Flexural modulus | 23.0 °C | 7.1 GPa Show Supplier Material materials with Flexural modulus of 7.1 GPa | ASTM D 790 | 2.6 mm/min, 100 mm span |
Flexural strength | 23.0 °C | 193 MPa Show Supplier Material materials with Flexural strength of 193 MPa | ASTM D 790 | brk, 2.6 mm/min, 100 mm span |
Tensile strength | 23.0 °C | 129 MPa Show Supplier Material materials with Tensile strength of 129 MPa | ASTM D 638 | yld, Type I, 5 mm/min |
Thermal
Property | Value | Comment | |
---|---|---|---|
Heat deflection temperature | 212 °C Show Supplier Material materials with Heat deflection temperature of 212 °C | ||
Heat deflection temperature, 1.80 MPa | 212 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 212 °C | ASTM D 648 | 6.4 mm, unannealed | |
Relative temperature index, electrical | 105 °C Show Supplier Material materials with Relative temperature index, electrical of 105 °C | UL 746B | |
Relative temperature index, mechanical impact | 105 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 105 °C | UL 746B | |
Relative temperature index, mechanical strength | 105 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 105 °C | UL 746B | |
Flammability | UL Recognized, 94V-0 Flame Class Rating: 1.5mm UL 94 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=524104- - |
Rheological Properties
Property | Value | Comment |
---|---|---|
Melt mass-flow rate | 10.3 g/10min Show Supplier Material materials with Melt mass-flow rate of 10.3 g/10min | ASTM D 1238 | 337°C/6.6 kgf |
Technological properties
Property | ||
---|---|---|
Application areas | Document Handling | |
Availability | Asia,Americas | |
Processing methods | Screw Speed: 40 to 70.0rpm | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |