General
Property | Temperature | Value | Comment |
---|---|---|---|
Density | 23.0 °C | 1.69 g/cm³ Show Supplier Material materials with Density of 1.69 g/cm³ | ISO 1183 |
Moisture absorption | 23.0 °C | 0.04 % Show Supplier Material materials with Moisture absorption of 0.04 % | ISO 62 | (23°C / 50% RH) |
Relative density | 23.0 °C | 1.69 [-] Show Supplier Material materials with Relative density of 1.69 [-] | ASTM D 792 | |
Water absorption | 23.0 °C | 0.1 % Show Supplier Material materials with Water absorption of 0.1 % | ISO 62-1 | (23°C/saturated) |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 14.7 GPa Show Supplier Material materials with Elastic modulus of 14.7 GPa | ISO 527 | 1 mm/min |
Elongation | 23.0 °C | 1.4 % Show Supplier Material materials with Elongation of 1.4 % | ISO 527 | break, 5 mm/min |
Flexural modulus | 23.0 °C | 13.6 GPa Show Supplier Material materials with Flexural modulus of 13.6 GPa | ISO 178 | 2 mm/min |
Flexural strength | 23.0 °C | 172 MPa Show Supplier Material materials with Flexural strength of 172 MPa | ISO 178 | yield, 2 mm/min |
Impact strength, Charpy notched | 23.0 °C | 4 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 4 kJ/m² | ISO 179/1eA | V-notch Edgew, 23°C, 80*10*4 sp=62mm |
Impact strength, Izod notched | 23.0 °C | 5 kJ/m² Show Supplier Material materials with Impact strength, Izod notched of 5 kJ/m² | ISO 180/1A | 80*10*4, -30°C |
Impact strength, Izod notched, ASTM | 23.0 °C | 49 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 49 J/m | ASTM D 256 | notched, -30°C |
Impact strength, Izod unnotched | 23.0 °C | 5 kJ/m² Show Supplier Material materials with Impact strength, Izod unnotched of 5 kJ/m² | ISO 180/1U | 80*10*4, 23°C |
Instrumented Impact, Total Energy | 23.0 °C | 12 J Show Supplier Material materials with Instrumented Impact, Total Energy of 12 J | ASTM D 3763 | 23°C |
Tensile strength | 23.0 °C | 121 MPa Show Supplier Material materials with Tensile strength of 121 MPa | ISO 527 | break, 5 mm/min |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Ball Pressure Test | Passes | IEC 60695-10-2 | 125°C +/- 2°C | |
Coefficient of thermal expansion | 23.0 °C | 1.6E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.6E-5 1/K | ISO 11359-2 | 23°C to 150°C |
Coefficient of thermal expansion, transverse | 23.0 °C | 3.8E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion, transverse of 3.8E-5 1/K | ISO 11359-2 | 23°C to 150°C |
Heat deflection temperature | 182 - 195 °C Show Supplier Material materials with Heat deflection temperature of 182 - 195 °C | ||
Heat deflection temperature, 0.45 MPa | 195 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 195 °C | ISO 75/Bf | Flatw 80*10*4 sp=64mm | |
Heat deflection temperature, 1.80 MPa | 182 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 182 °C | ISO 75/Af | Flatw 80*10*4 sp=64mm | |
Vicat softening temperature | 195 °C Show Supplier Material materials with Vicat softening temperature of 195 °C | ISO 306 | Rate B/120 |
Electrical
Property | Temperature | Value | Comment |
---|---|---|---|
Sheet resistivity, ROA | 23.0 °C | 2.10E+15 Ω Show Supplier Material materials with Sheet resistivity, ROA of 2.10E+15 Ω | ASTM D 257 |
Volume resistivity | 23.0 °C | 6.00E+15 Ω·cm Show Supplier Material materials with Volume resistivity of 6.00E+15 Ω·cm | ASTM D 257 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Melt mass-flow rate | 20 g/10min Show Supplier Material materials with Melt mass-flow rate of 20 g/10min | ASTM D 1238 | 337°C/6.6 kgf | |
Melt volume-flow rate | 20 cm³/10min Show Supplier Material materials with Melt volume-flow rate of 20 cm³/10min | ISO 1133 | MVR at 360°C/5.0 kg | |
Shrinkage | 23.0 °C | 0.2 % Show Supplier Material materials with Shrinkage of 0.2 % | SABIC method | 3.2 mm |
Shrinkage, transverse | 23.0 °C | 0.3 % Show Supplier Material materials with Shrinkage, transverse of 0.3 % | SABIC method | 3.2 mm |
Technological properties
Property | ||
---|---|---|
Availability | Europe,Asia,Americas | |
Processing methods | Drying Time: 4 to 6.0hrs | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |