20% Glass fiber filled, enhanced flow Polyetherimide (Tg 217C). ECO Conforming. For medical devices and pharmaceutical applications. Healthcare management of change, biocompatible (ISO 10993 or USP Class VI); food contact compliant; Steam, Gamma, EtO, and E-beam sterilizable.

This material data has been provided by Sabic.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.42 g/cm³

Show Supplier Material materials with Density of 1.42 g/cm³

ISO 1183

Moisture absorption

23.0 °C

0.55 %

Show Supplier Material materials with Moisture absorption of 0.55 %

ISO 62 | (23°C / 50% RH)

Relative density

23.0 °C

1.42 [-]

Show Supplier Material materials with Relative density of 1.42 [-]

ASTM D 792

Water absorption

23.0 °C

1 %

Show Supplier Material materials with Water absorption of 1 %

ISO 62-1 | (23°C/saturated)

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

6.9 GPa

Show Supplier Material materials with Elastic modulus of 6.9 GPa

ISO 527 | 1 mm/min

Elongation

23.0 °C

4 %

Show Supplier Material materials with Elongation of 4 %

ISO 527 | break, 5 mm/min

Flexural modulus

23.0 °C

6.9 GPa

Show Supplier Material materials with Flexural modulus of 6.9 GPa

ISO 178 | 2 mm/min

Flexural strength

23.0 °C

228 MPa

Show Supplier Material materials with Flexural strength of 228 MPa

ISO 178 | yield, 2 mm/min

Impact strength, Charpy notched

23.0 °C

65 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 65 kJ/m²

ISO 179/1eA | V-notch Edgew 80*10*4 sp=62mm, 23°C

Impact strength, Izod notched

23.0 °C

64 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 64 kJ/m²

ISO 180/1A | 80*10*4, 23°C

Impact strength, Izod notched, ASTM

23.0 °C

70 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 70 J/m

ASTM D 256

Impact strength, Izod unnotched, ASTM

23.0 °C

480 J/m

Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 480 J/m

ASTM D 4812 | 23°C

Instrumented Impact, Total Energy

23.0 °C

8 J

Show Supplier Material materials with Instrumented Impact, Total Energy of 8 J

ASTM D 3763 | 23°C

Tensile strength

23.0 °C

131 MPa

Show Supplier Material materials with Tensile strength of 131 MPa

ISO 527 | break, 5 mm/min

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

2.5E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 2.5E-5 1/K

ISO 11359-2 | 23°C to 150°C

Coefficient of thermal expansion, transverse

23.0 °C

5E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion, transverse of 5E-5 1/K

ISO 11359-2 | 23°C to 150°C

Heat deflection temperature

205 °C

Show Supplier Material materials with Heat deflection temperature of 205 °C

Heat deflection temperature, 1.80 MPa

205 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 205 °C

ISO 75/Ae | Edgew 120*10*4 sp=100mm

Relative temperature index, electrical

170 °C

Show Supplier Material materials with Relative temperature index, electrical of 170 °C

UL 746B

Relative temperature index, mechanical impact

170 °C

Show Supplier Material materials with Relative temperature index, mechanical impact of 170 °C

UL 746B

Relative temperature index, mechanical strength

170 °C

Show Supplier Material materials with Relative temperature index, mechanical strength of 170 °C

UL 746B

Vicat softening temperature

218 °C

Show Supplier Material materials with Vicat softening temperature of 218 °C

ISO 306 | Rate B/120

Flammability

UL Recognized, 94-5VA Flame Class Rating: ≥1.9mm UL 94 <br> UL Recognized, 94V-0 Flame Class Rating: ≥0.41mm UL 94 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=221093- -

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

4 V

Show Supplier Material materials with Comparative tracking index of 4 V

UL 746A | (UL) {PLC}

High Amp Arc Ignition

23.0 °C

1.5 mm

Show Supplier Material materials with High Amp Arc Ignition of 1.5 mm

≥, UL 746A | PLC 3

High Volt Arc Track Rate

23.0 °C

2 PLC Code

Show Supplier Material materials with High Volt Arc Track Rate of 2 PLC Code

UL 746A | (PLC)

Hot-Wire Ignition

23.0 °C

3 mm

Show Supplier Material materials with Hot-Wire Ignition of 3 mm

≥, UL 746A | PLC 1

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

6 g/10min

Show Supplier Material materials with Melt mass-flow rate of 6 g/10min

ASTM D 1238 | 337°C/6.6 kgf

Melt volume-flow rate

7 cm³/10min

Show Supplier Material materials with Melt volume-flow rate of 7 cm³/10min

ISO 1133 | MVR at 360°C/5.0 kg

Shrinkage

23.0 °C

0.3 %

Show Supplier Material materials with Shrinkage of 0.3 %

SABIC method | 3.2 mm

Technological properties

Property
Application areas

Surgical Devices

Availability

Americas

Processing methods

Vent Depth: 0.025 to 0.076mm
Drying Time: 4 to 6.0hrs
Middle - Zone 2 Temperature: 340 to 400.0°C
Back Pressure: 0.3 to 0.7MPa
Rear - Zone 1 Temperature: 330 to 400.0°C
Nozzle Temperature: 345 to 400.0°C
Maximum Moisture Content: 0.02%
Melt Temperature: 350 to 400.0°C
Mold Temperature: 135 to 165.0°C
Shot to Cylinder Size: 40 to 60.0%
Front - Zone 3 Temperature: 345 to 400.0°C
Drying Temperature: 150°C
Drying Time (Cumulative): 24hrs
Screw Speed: 40 to 70.0rpm

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.