Description

Transparent, Standard flow Polyetherimide copolymer (Tg 225C) with enhanced chemical resistance to strong acids, bases, aromatics, and ketones. ECO conforming, UL94 V0 listing.

This material data has been provided by Sabic.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyTemperatureValueComment

Water absorption

23.0 °C

1.2 %

Show Supplier Material materials with Water absorption of 1.2 %

ISO 62-1 | (23°C/saturated)

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

3.2 GPa

Show Supplier Material materials with Elastic modulus of 3.2 GPa

ISO 527 | 1 mm/min

Elongation

23.0 °C

50 %

Show Supplier Material materials with Elongation of 50 %

ISO 527 | break, 50 mm/min

Flexural modulus

23.0 °C

2.5 GPa

Show Supplier Material materials with Flexural modulus of 2.5 GPa

ISO 178 | 2 mm/min

Flexural strength

23.0 °C

110 MPa

Show Supplier Material materials with Flexural strength of 110 MPa

ISO 178 | yield, 2 mm/min

Impact strength, Izod notched

23.0 °C

8 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 8 kJ/m²

ISO 180/1A | notched 80*10*4, -30°C

Tensile strength

23.0 °C

95 MPa

Show Supplier Material materials with Tensile strength of 95 MPa

ISO 527 | break, 50 mm/min

Thermal

PropertyValueComment

Heat deflection temperature, 1.80 MPa

200 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 200 °C

ISO 75/Ae | Edgew 120*10*4 sp=100mm

Relative temperature index, electrical

160 °C

Show Supplier Material materials with Relative temperature index, electrical of 160 °C

UL 746B

Relative temperature index, mechanical impact

160 °C

Show Supplier Material materials with Relative temperature index, mechanical impact of 160 °C

UL 746B

Relative temperature index, mechanical strength

160 °C

Show Supplier Material materials with Relative temperature index, mechanical strength of 160 °C

UL 746B

Flammability

UL Recognized, 94V-0 Flame Class Rating: ≥1.5mm UL 94 <br> Glow Wire Flammability Index 960°C, passes at: 3.2mm IEC 60695-2-12 <br> Glow Wire Flammability Index 960°C, passes at: 3.2mm IEC 60695-2-12 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=221114- -

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

4 V

Show Supplier Material materials with Comparative tracking index of 4 V

UL 746A | (UL) {PLC}

Dielectric strength

23.0 °C

26 kV/mm

Show Supplier Material materials with Dielectric strength of 26 kV/mm

IEC 60243-1 | in oil, 1.6 mm

High Amp Arc Ignition

23.0 °C

1.5 mm

Show Supplier Material materials with High Amp Arc Ignition of 1.5 mm

≥, UL 746A | PLC 0

High Volt Arc Track Rate

23.0 °C

3 PLC Code

Show Supplier Material materials with High Volt Arc Track Rate of 3 PLC Code

UL 746A | (PLC)

Hot-Wire Ignition

23.0 °C

1.5 mm

Show Supplier Material materials with Hot-Wire Ignition of 1.5 mm

≥, UL 746A | PLC 0

Sheet resistivity, ROA

23.0 °C

1.00E+15 Ω

Show Supplier Material materials with Sheet resistivity, ROA of 1.00E+15 Ω

>, IEC 60093

Volume resistivity

23.0 °C

1.00E+15 Ω·cm

Show Supplier Material materials with Volume resistivity of 1.00E+15 Ω·cm

IEC 60093 |

Rheological Properties

PropertyTemperatureValueComment

Shrinkage

23.0 °C

0.6 %

Show Supplier Material materials with Shrinkage of 0.6 %

SABIC method | on tensile bar

Technological properties

Property
Application areas

Medical Device, LED Lighting, Meter Water, Photovoltaic Components, Semiconductor, Wireless Communications, Audio, Aerospace, Air Cabin Interiors, Electronic Components, Enclosure/Housing/Cover, Energy Management, Enclosures, Industrial Material Handling, Heavy Vehicles

Availability

Europe,Asia,Americas

Features

High Stiffness, Hydrolytic Stability, Enhanced Chemical Resistance, Low Smoke and Toxicity, Good Mechanicals in Broad Temperature Range, Low Creep Sensitivity, Low Shrinkage, Good metal adhesion, Amorphous, High Strength, High Heat Resistance, Good dimensional stability, Flame Retardant, Transparent

Processing methods

Melt Temperature: 360 to 410.0°C
Maximum Moisture Content: 0.02%
Drying Time: 4 to 6.0hrs
Front - Zone 3 Temperature: 370 to 410.0°C
Hopper Temperature: 80 to 120.0°C
Rear - Zone 1 Temperature: 325 to 365.0°C
Nozzle Temperature: 360 to 400.0°C
Drying Temperature: 150°C
Middle - Zone 2 Temperature: 350 to 390.0°C
Mold Temperature: 120 to 170.0°C

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.