Description

20% Glass fiber filled, enhanced flow Polyetherimide (Tg 217C) with internal mold release. ECO Conforming, UL94 V0 and 5VA listing.

This material data has been provided by Sabic.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyTemperatureValueComment

Limiting oxygen index

23.0 °C

50 %

Show Supplier Material materials with Limiting oxygen index of 50 %

Relative density

23.0 °C

1.42 [-]

Show Supplier Material materials with Relative density of 1.42 [-]

ASTM D 792

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

6.89 GPa

Show Supplier Material materials with Elastic modulus of 6.89 GPa

ASTM D 638 | 5 mm/min

Elongation

23.0 °C

4 %

Show Supplier Material materials with Elongation of 4 %

ASTM D 638 | brk, Type I, 5 mm/min

Flexural modulus

23.0 °C

6.89 GPa

Show Supplier Material materials with Flexural modulus of 6.89 GPa

ASTM D 790 | 2.6 mm/min, 100 mm span

Flexural strength

23.0 °C

227 MPa

Show Supplier Material materials with Flexural strength of 227 MPa

ASTM D 790 | brk, 2.6 mm/min, 100 mm span

Impact strength, Izod notched

23.0 °C

74 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 74 kJ/m²

ASTM D 256 | notched, 23°C

Impact strength, Izod notched, ASTM

23.0 °C

74 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 74 J/m

ASTM D 256

Impact strength, Izod unnotched, ASTM

23.0 °C

475 J/m

Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 475 J/m

ASTM D 4812 | 23°C

Tensile strength

23.0 °C

139 MPa

Show Supplier Material materials with Tensile strength of 139 MPa

ASTM D 638 | brk, Type I, 5 mm/min

Thermal

PropertyValueComment

Heat deflection temperature, 0.45 MPa

210 °C

Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 210 °C

ASTM D 648 | 6.4 mm, unannealed

Heat deflection temperature, 1.80 MPa

211 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 211 °C

ASTM D 648 | 6.4 mm, unannealed

Relative temperature index, electrical

170 °C

Show Supplier Material materials with Relative temperature index, electrical of 170 °C

UL 746B

Relative temperature index, mechanical impact

170 °C

Show Supplier Material materials with Relative temperature index, mechanical impact of 170 °C

UL 746B

Relative temperature index, mechanical strength

170 °C

Show Supplier Material materials with Relative temperature index, mechanical strength of 170 °C

UL 746B

Vicat softening temperature

225 °C

Show Supplier Material materials with Vicat softening temperature of 225 °C

ASTM D 1525 | Rate B/50

Flammability

UL Recognized, 94V-0 Flame Class Rating: ≥0.41mm UL 94 <br> UL Recognized, 94-5VA Flame Class Rating: ≥1.9mm UL 94 <br> UV-light, water exposure/immersion: F1- UL 746C <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=221093- - <br> UL Yellow Card Link 2: https://iq.ul.com/ul/cert.aspx?ULID=502535- -

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

4 V

Show Supplier Material materials with Comparative tracking index of 4 V

UL 746A | (UL) {PLC}

High Amp Arc Ignition

23.0 °C

3 mm

Show Supplier Material materials with High Amp Arc Ignition of 3 mm

≥, UL 746A | PLC 4

High Volt Arc Track Rate

23.0 °C

2 PLC Code

Show Supplier Material materials with High Volt Arc Track Rate of 2 PLC Code

UL 746A | (PLC)

Hot-Wire Ignition

23.0 °C

1.5 mm

Show Supplier Material materials with Hot-Wire Ignition of 1.5 mm

≥, UL 746A | PLC 2

Technological properties

Property
Application areas

Enclosure/Housing/Cover, Electronic Components, Lab Ware and Clinical Diagnostics, Displays, Document Handling, Data Management, Data Transfer, Circuit Protection, Audio, Aerospace, Additive Semiconductor Materials, Personal Computing, Personal Care, Semiconductor, Wiring Devices, Wireless Communications, Tray, Wire & cable

Availability

Europe,Asia,Americas

Features

High Stiffness, Hydrolytic Stability, Chemical Resistance, Easy Flow, Low Smoke and Toxicity, Good Mechanicals in Broad Temperature Range, Low Creep Sensitivity, Low Shrinkage, Good metal adhesion, Amorphous, High Strength, General Purpose, High Heat Resistance, Good dimensional stability, Flame Retardant, Good Mold Release

Processing methods

Screw Speed: 40 to 70.0rpm
Vent Depth: 0.025 to 0.076mm
Nozzle Temperature: 345 to 400.0°C
Melt Temperature: 350 to 400.0°C
Shot to Cylinder Size: 40 to 60.0%
Back Pressure: 0.3 to 0.7MPa
Maximum Moisture Content: 0.02%
Mold Temperature: 135 to 165.0°C
Drying Temperature: 150°C
Rear - Zone 1 Temperature: 330 to 400.0°C
Front - Zone 3 Temperature: 345 to 400.0°C
Drying Time (Cumulative): 24hrs
Drying Time: 4 to 6.0hrs
Middle - Zone 2 Temperature: 340 to 400.0°C

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.