Description

NORYL™ N110 resin is a non-reinforced blend of polyphenylene ether (PPE) + high impact polystyrene (HIPS). This impact modified, injection moldable grade was developed for automotive body panel applications and meets the requirements of the Standard ECE Dashboard Impact Test. NORYL N110 resin offers heat resistance, good impact resistance, low specific gravity, and dimensional stability. It is an excellent candidate for a variety of automotive instrument panel applications.

This material data has been provided by Sabic.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.05 g/cm³

Show Supplier Material materials with Density of 1.05 g/cm³

ISO 1183

Limiting oxygen index

23.0 °C

19 %

Show Supplier Material materials with Limiting oxygen index of 19 %

Moisture absorption

23.0 °C

0.07 %

Show Supplier Material materials with Moisture absorption of 0.07 %

ISO 62 | (23°C / 50% RH)

Water absorption

23.0 °C

0.2 %

Show Supplier Material materials with Water absorption of 0.2 %

ISO 62-1 | (23°C/saturated)

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

2.2 GPa

Show Supplier Material materials with Elastic modulus of 2.2 GPa

ISO 527 | 1 mm/min

Elongation

23.0 °C

30 %

Show Supplier Material materials with Elongation of 30 %

ISO 527 | break, 50 mm/min

Flexural modulus

23.0 °C

2 GPa

Show Supplier Material materials with Flexural modulus of 2 GPa

ISO 178 | 2 mm/min

Flexural strength

23.0 °C

60 MPa

Show Supplier Material materials with Flexural strength of 60 MPa

ISO 178 | yield, 2 mm/min

Hardness, Ball Indentation

23.0 °C

95 MPa

Show Supplier Material materials with Hardness, Ball Indentation of 95 MPa

ISO 2039-1 | H358/30

Impact strength, Charpy notched

23.0 °C

5 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 5 kJ/m²

ISO 179/1eA | V-notch Edgew 80*10*4 sp=62mm, -30°C

Impact strength, Izod notched

23.0 °C

11 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 11 kJ/m²

ISO 180/1A | 80*10*4, 23°C

Tensile strength

23.0 °C

45 MPa

Show Supplier Material materials with Tensile strength of 45 MPa

ISO 527 | yield, 50 mm/min

Thermal

PropertyTemperatureValueComment

Ball Pressure Test

nan

IEC 60695-10-2 | 75°C +/- 2°C

Ball pressure temperature

115 °C

Show Supplier Material materials with Ball pressure temperature of 115 °C

IEC 60695-10-2 | approximate maximum

Coefficient of thermal expansion

23.0 °C

7E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 7E-5 1/K

ISO 11359-2 | 23°C to 80°C

Coefficient of thermal expansion, transverse

23.0 °C

9E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion, transverse of 9E-5 1/K

ISO 11359-2 | 23°C to 80°C

Heat deflection temperature

95 - 105 °C

Show Supplier Material materials with Heat deflection temperature of 95 - 105 °C

Heat deflection temperature, 0.45 MPa

105 °C

Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 105 °C

ISO 75/Be | Edgew 120*10*4 sp=100mm

Heat deflection temperature, 1.80 MPa

95 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 95 °C

ISO 75/Ae | Edgew 120*10*4 sp=100mm

Relative temperature index, electrical

90 °C

Show Supplier Material materials with Relative temperature index, electrical of 90 °C

UL 746B

Relative temperature index, mechanical impact

85 °C

Show Supplier Material materials with Relative temperature index, mechanical impact of 85 °C

UL 746B

Relative temperature index, mechanical strength

95 °C

Show Supplier Material materials with Relative temperature index, mechanical strength of 95 °C

UL 746B

Thermal conductivity

23.0 °C

0.22 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 0.22 W/(m·K)

ISO 8302

Vicat softening temperature

115 °C

Show Supplier Material materials with Vicat softening temperature of 115 °C

ISO 306 | Rate B/120

Flammability

Glow Wire Flammability Index 960°C, passes at: 3.2mm IEC 60695-2-12 <br> Glow Wire Flammability Index 960°C, passes at: 3.2mm IEC 60695-2-12 <br> UL Recognized, 94HB Flame Class Rating: ≥1.5mm UL 94 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=236761- -

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

2 V

Show Supplier Material materials with Comparative tracking index of 2 V

UL 746A | (UL) {PLC}

Dielectric constant, 1MHz

23.0 °C

2.6 [-]

Show Supplier Material materials with Dielectric constant, 1MHz of 2.6 [-]

IEC 60250

Dielectric constant, 60Hz

23.0 °C

2.6 [-]

Show Supplier Material materials with Dielectric constant, 60Hz of 2.6 [-]

IEC 60250 | 50/60 Hz

Dielectric strength

23.0 °C

19 kV/mm

Show Supplier Material materials with Dielectric strength of 19 kV/mm

IEC 60243-1 | in oil, 3.2 mm,

Dissipation factor, 1MHz

23.0 °C

1E-3 [-]

Show Supplier Material materials with Dissipation factor, 1MHz of 1E-3 [-]

IEC 60250

Dissipation factor, 50Hz

23.0 °C

4E-3 [-]

Show Supplier Material materials with Dissipation factor, 50Hz of 4E-3 [-]

IEC 60250 | 50/60 Hz

High Amp Arc Ignition

23.0 °C

1.5 mm

Show Supplier Material materials with High Amp Arc Ignition of 1.5 mm

≥, UL 746A | PLC 0

High Volt Arc Track Rate

23.0 °C

3 PLC Code

Show Supplier Material materials with High Volt Arc Track Rate of 3 PLC Code

UL 746A | (PLC)

Hot-Wire Ignition

23.0 °C

1.5 mm

Show Supplier Material materials with Hot-Wire Ignition of 1.5 mm

≥, UL 746A | PLC 3

Sheet resistivity, ROA

23.0 °C

1.00E+15 Ω

Show Supplier Material materials with Sheet resistivity, ROA of 1.00E+15 Ω

>, IEC 60093

Volume resistivity

23.0 °C

1.00E+15 Ω·cm

Show Supplier Material materials with Volume resistivity of 1.00E+15 Ω·cm

IEC 60093 |

Rheological Properties

PropertyTemperatureValueComment

Melt volume-flow rate

15 cm³/10min

Show Supplier Material materials with Melt volume-flow rate of 15 cm³/10min

ISO 1133 | MVR at 280°C/3.8 kg

Shrinkage

23.0 °C

0.5 %

Show Supplier Material materials with Shrinkage of 0.5 %

SABIC method | on tensile bar

Technological properties

Property
Application areas

Personal Computing, Meter Water, Photovoltaic Components, Plumbing, Pharmaceutical Packaging & Drug Delivery, Refrigerator, Pump, Wheel Cover, Wiring Devices, Swimming Pool/Spa, Bottles, Cladding/Roof, Data Transfer, Circuit Protection, Electronic Components, Energy Management, Enclosures, Freezer, Heavy Vehicles, Lab Ware and Clinical Diagnostics

Availability

Europe

Features

Hydrolytic Stability, Low Creep Sensitivity

Processing methods

Nozzle Temperature: 260 to 280.0°C
Rear - Zone 1 Temperature: 240 to 260.0°C
Drying Time: 2 to 4.0hrs
Middle - Zone 2 Temperature: 260 to 280.0°C
Drying Temperature: 80 to 100.0°C
Mold Temperature: 60 to 100.0°C
Front - Zone 3 Temperature: 280 to 300.0°C
Hopper Temperature: 60 to 80.0°C
Melt Temperature: 280 to 300.0°C

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.