NORYL™ Resin LS6010 - Europe

Want to keep this datasheet? Save it now in your required format

Description

NORYL™ LS6010 resin is a non-reinforced blend of polyphenylene ether (PPE) + high impact polystyrene (HIPS). This high performance, injection moldable and extrudable grade contains non-brominated, non-chlorinated flame retardant and carries a UL94 flame rating of V0 at 1.5mm. NORYL LS6010 resin features low smoke production upon burning, high heat resistance, very low specific gravity, enhanced resistance to melting and dripping and meets the requirements of FAR 25.853. In addition, this material is heat stabilized and impact modified. It is an excellent candidate for aerospace interior applications such as rub strips, seat track covers, cable guides, switch panels, conduit, wall/ceiling mounted electronics, and parts machined from slab stock.

This material data has been provided by Sabic.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.11 g/cm³

Show Supplier Material materials with Density of 1.11 g/cm³

ISO 1183

Moisture absorption

23.0 °C

0.05 %

Show Supplier Material materials with Moisture absorption of 0.05 %

ISO 62 | (23°C / 50% RH)

Relative density

23.0 °C

1.11 [-]

Show Supplier Material materials with Relative density of 1.11 [-]

ASTM D 792 |

Water absorption

23.0 °C

0.2 %

Show Supplier Material materials with Water absorption of 0.2 %

ISO 62-1 | (23°C/saturated)

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

2.44 GPa

Show Supplier Material materials with Elastic modulus of 2.44 GPa

ISO 527 | 1 mm/min

Elongation

23.0 °C

4.7 %

Show Supplier Material materials with Elongation of 4.7 %

ISO 527 | yield, 50 mm/min

Flexural modulus

23.0 °C

2.36 GPa

Show Supplier Material materials with Flexural modulus of 2.36 GPa

ISO 178 | 2 mm/min

Flexural strength

23.0 °C

100 MPa

Show Supplier Material materials with Flexural strength of 100 MPa

ISO 178 | yield, 2 mm/min

Impact strength, Charpy notched

23.0 °C

20 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 20 kJ/m²

ISO 179/1eA | V-notch Edgew, 23°C, 80*10*4 sp=62mm

Impact strength, Izod notched

23.0 °C

14 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 14 kJ/m²

ISO 180/1A | 80*10*4, -30°C

Impact strength, Izod notched, ASTM

23.0 °C

181 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 181 J/m

ASTM D 256

Instrumented Impact, Total Energy

23.0 °C

52 J

Show Supplier Material materials with Instrumented Impact, Total Energy of 52 J

ASTM D 3763 | 23°C

Tensile strength

23.0 °C

58 MPa

Show Supplier Material materials with Tensile strength of 58 MPa

ISO 527 | break, 50 mm/min

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

6.7E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 6.7E-5 1/K

ISO 11359-2 | -40°C to 40°C

Coefficient of thermal expansion, transverse

23.0 °C

6.7E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion, transverse of 6.7E-5 1/K

ISO 11359-2 | -40°C to 40°C

Heat deflection temperature, 1.80 MPa

124 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 124 °C

ISO 75/Af | Flatw 80*10*4 sp=64mm

Vicat softening temperature

143 °C

Show Supplier Material materials with Vicat softening temperature of 143 °C

ISO 306 | Rate B/50

Flammability

Vertical Burn b (12s, 1.52mm) passes at: 4sec FAR 25.853 <br> Vertical Burn a (60s, 1.52mm) passes at: 0sec FAR 25.853 <br> Flame Spread Index (1.52mm): 15- ASTM E 162 <br> NBS Smoke Density, Non-Flaming, 4 min (1.52mm): 7- ASTM E 662 <br> NBS Smoke Density, Flaming, 4 min (1.52mm): 30- ASTM E 662 <br> Draeger Tube Toxicity, Flaming (1.52mm): Pass- Based on ASTM E 662 <br> Draeger Tube Toxicity, Non-Flaming (1.52mm): Pass- Based on ASTM E 662

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

5.6 g/10min

Show Supplier Material materials with Melt mass-flow rate of 5.6 g/10min

ASTM D 1238 | 280°C/5.0 kgf

Melt volume-flow rate

5 cm³/10min

Show Supplier Material materials with Melt volume-flow rate of 5 cm³/10min

ISO 1133 | MVR at 280°C/5.0 kg

Shrinkage

23.0 °C

0.5 %

Show Supplier Material materials with Shrinkage of 0.5 %

SABIC method | 3.2 mm

Technological properties

Property
Application areas

Air Cabin Interiors, Aerospace, Aircraft Seating, Interior Rail Components

Availability

Europe,Asia,Americas

Features

Hydrolytic Stability, Low Creep Sensitivity, Flame Retardant, Non-Halogenated, Non-Brominated, Low Warpage

Processing methods

Shot to Cylinder Size: 30 to 70.0%
Maximum Moisture Content: 0.07%
Barrel - Zone 2 Temperature: 220 to 260.0°C
Drying Time (Cumulative): 12hrs
Mold Temperature: 65 to 100.0°C
Drying Time: 2 to 4.0hrs
Roll Stack Temp - Middle: 90 to 150.0°C
Middle - Zone 2 Temperature: 290 to 300.0°C
Die Temperature: 220 to 260.0°C
Drying Temperature: 95 to 105.0°C
Nozzle Temperature: 295 to 305.0°C
Front - Zone 3 Temperature: 295 to 305.0°C
Adapter Temperature: 220 to 260.0°C
Roll Stack Temp - Bottom: 90 to 150.0°C
Roll Stack Temp - Top: 90 to 150.0°C
Drying Time (Cumulative): 12hrs
Barrel - Zone 3 Temperature: 220 to 260.0°C
Drying Time (Cumulative): 12hrs
Barrel - Zone 3 Temperature: 220 to 260.0°C
Barrel - Zone 2 Temperature: 220 to 260.0°C
Barrel - Zone 1 Temperature: 220 to 260.0°C
Calibrator Temperature: 30 to 60.0°C
Drying Temperature: 95 to 105.0°C
Drying Temperature: 95 to 105.0°C
Melt Temperature: 220 to 260.0°C
Hopper Temperature: 80 to 120.0°C
Melt Temperature: 280 to 305.0°C
Die Temperature: 220 to 260.0°C
Adapter Temperature: 220 to 260.0°C
Barrel - Zone 4 Temperature: 220 to 260.0°C
Rear - Zone 1 Temperature: 280 to 295.0°C
Screw Speed: 40 to 80.0rpm
Barrel - Zone 1 Temperature: 220 to 260.0°C
Maximum Moisture Content: 0.07%
Melt Temperature: 220 to 260.0°C
Drying Time: 2 to 4.0hrs
Barrel - Zone 4 Temperature: 220 to 260.0°C
Drying Time: 2 to 4.0hrs
Water Bath Temperature: 30 to 50.0°C

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.