NORYL GTX™ Resin GTX678 - Asia

Want to keep this datasheet? Save it now in your required format

Description

NORYL GTX™ 678 resin is a conductive, high performance non-reinforced alloy of Polyphenylene Ether (PPE) + Polyamide (PA). This injection moldable grade is optimized for primer-less electrostatic and powder coat painting, and it is UL 5VA rated with a non-brominated, non-chlorinated FR package. NORYL GTX678 resin exhibits an excellent balance of conductivity, high heat resistance, good ductility, and is heat stabilized. This material is an excellent candidate for non-automotive painted applications such as office furniture, PVC/metal replacement, lighting ballast housings / enclosures, and appliance exteriors.

This material data has been provided by Sabic.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.12 g/cm³

Show Supplier Material materials with Density of 1.12 g/cm³

ISO 1183

Moisture absorption

23.0 °C

0.5 %

Show Supplier Material materials with Moisture absorption of 0.5 %

ISO 62 | (23°C / 50% RH)

Relative density

23.0 °C

1.12 [-]

Show Supplier Material materials with Relative density of 1.12 [-]

ASTM D 792 |

Water absorption

23.0 °C

4 %

Show Supplier Material materials with Water absorption of 4 %

ISO 62-1 | (23°C/saturated)

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

2.9 GPa

Show Supplier Material materials with Elastic modulus of 2.9 GPa

ISO 527 | 1 mm/min

Elongation

23.0 °C

7 %

Show Supplier Material materials with Elongation of 7 %

ISO 527 | yield, 50 mm/min

Flexural modulus

23.0 °C

2.6 GPa

Show Supplier Material materials with Flexural modulus of 2.6 GPa

ISO 178 | 2 mm/min

Flexural strength

23.0 °C

95 MPa

Show Supplier Material materials with Flexural strength of 95 MPa

ISO 178 | yield, 2 mm/min

Impact strength, Charpy notched

23.0 °C

12 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 12 kJ/m²

ISO 179/1eA | V-notch Edgew 80*10*4 sp=62mm, 23°C

Impact strength, Izod notched

23.0 °C

10 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 10 kJ/m²

ISO 180/1A | notched 80*10*4, 23°C

Impact strength, Izod notched, ASTM

23.0 °C

70 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 70 J/m

ASTM D 256

Instrumented Impact, Total Energy

23.0 °C

60 J

Show Supplier Material materials with Instrumented Impact, Total Energy of 60 J

ASTM D 3763 | 23°C

Tensile strength

23.0 °C

52 MPa

Show Supplier Material materials with Tensile strength of 52 MPa

ISO 527 | break, 50 mm/min

Thermal

PropertyTemperatureValueComment

Ball Pressure Test

PASS

IEC 60695-10-2 | 125°C +/- 2°C

Coefficient of thermal expansion

23.0 °C

8.3E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 8.3E-5 1/K

ISO 11359-2 | 23°C to 60°C

Coefficient of thermal expansion, transverse

23.0 °C

8.5E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion, transverse of 8.5E-5 1/K

ISO 11359-2 | 23°C to 60°C

Heat deflection temperature

191 °C

Show Supplier Material materials with Heat deflection temperature of 191 °C

Heat deflection temperature, 0.45 MPa

191 °C

Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 191 °C

ISO 75/Bf | Flatw 80*10*4 sp=64mm

Specific heat capacity

23.0 °C

1.4E-3 J/(kg·K)

Show Supplier Material materials with Specific heat capacity of 1.4E-3 J/(kg·K)

ASTM C 351

Thermal conductivity

23.0 °C

0.2 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 0.2 W/(m·K)

ASTM C177

Vicat softening temperature

195 °C

Show Supplier Material materials with Vicat softening temperature of 195 °C

ISO 306 | Rate B/120

Electrical

PropertyTemperatureValueComment

Volume resistivity

23.0 °C

4000 Ω·cm

Show Supplier Material materials with Volume resistivity of 4000 Ω·cm

ASTM D 257

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

7.8 g/10min

Show Supplier Material materials with Melt mass-flow rate of 7.8 g/10min

ASTM D 1238 | 300°C/5.0 kgf

Melt volume-flow rate

7 cm³/10min

Show Supplier Material materials with Melt volume-flow rate of 7 cm³/10min

ISO 1133 | MVR at 300°C/5.0 kg

Shrinkage

23.0 °C

1.3 %

Show Supplier Material materials with Shrinkage of 1.3 %

SABIC method | 3.2 mm

Technological properties

Property
Application areas

Head Protection, Circuit Protection

Availability

Europe,Asia,Americas

Features

Hydrolytic Stability, Chemical Resistance, Good Stiffness, Low Warpage, Heat Stabilized, Conductive, Structural

Processing methods

Barrel - Zone 4 Temperature: 245 to 260.0°C
Melt Temperature: 245 to 260.0°C
Vent Depth: 0.013 to 0.038mm
Mold Temperature: 65 to 95.0°C
Back Pressure: 0.3 to 1.4MPa
Minimum Moisture Content: 0.02%
Barrel - Zone 3 Temperature: 245 to 260.0°C
Nozzle Temperature: 275 to 300.0°C
Middle - Zone 2 Temperature: 265 to 300.0°C
Adapter Temperature: 245 to 260.0°C
Rear - Zone 1 Temperature: 260 to 300.0°C
Drying Temperature: 105 to 110.0°C
Front - Zone 3 Temperature: 270 to 300.0°C
Drying Time: 8hrs
Maximum Moisture Content: 0.07%
Screw Speed: 20 to 100.0rpm
Drying Time (Cumulative): 24hrs
Maximum Moisture Content: 0.03%
Barrel - Zone 1 Temperature: 245 to 260.0°C
Drying Time (Cumulative): 8hrs
Calibrator Temperature: 35 to 75.0°C
Drying Time: 3 to 4.0hrs
Drying Temperature: 95 to 105.0°C
Melt Temperature: 275 to 300.0°C
Barrel - Zone 2 Temperature: 245 to 260.0°C
Shot to Cylinder Size: 30 to 50.0%
Die Temperature: 245 to 260.0°C
Water Bath Temperature: 40 - 50°C

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.