ULTEM™ Resin AUR200G6 - Europe

Want to keep this datasheet? Save it now in your required format

Description

AUR200G6 is a 30 percent glass filled ULTEM Utility grade. The grade will have a limited color availabilty, dark gray to black. The data listed in this data sheet are the lower specification limits, apart from the MFR, CTE, HDT at 1.8 MPa, Density, Tensile strain, Water Absorption, Thermal Conductivity and Shrinkage which are typical data. The MVR of this material at 337 degrees C/6.7 kgf will have a specification between 3 and 7.5 (MFR: 4.2-10.5)

This material data has been provided by Sabic.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.53 g/cm³

Show Supplier Material materials with Density of 1.53 g/cm³

ISO 1183

Moisture absorption

23.0 °C

0.5 %

Show Supplier Material materials with Moisture absorption of 0.5 %

ISO 62 | (23°C / 50% RH)

Water absorption

23.0 °C

0.9 %

Show Supplier Material materials with Water absorption of 0.9 %

ISO 62-1 | (23°C/saturated)

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

8 GPa

Show Supplier Material materials with Elastic modulus of 8 GPa

ISO 527 | 1 mm/min

Elongation

23.0 °C

3 %

Show Supplier Material materials with Elongation of 3 %

ISO 527 | break, 5 mm/min

Flexural modulus

23.0 °C

6.5 GPa

Show Supplier Material materials with Flexural modulus of 6.5 GPa

ISO 178 | 2 mm/min

Flexural strength

23.0 °C

180 MPa

Show Supplier Material materials with Flexural strength of 180 MPa

ISO 178 | yield, 2 mm/min

Impact strength, Izod notched

23.0 °C

4 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 4 kJ/m²

ISO 180/1A | 80*10*4, 23°C

Tensile strength

23.0 °C

120 MPa

Show Supplier Material materials with Tensile strength of 120 MPa

ISO 527 | break, 5 mm/min

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

2.5E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 2.5E-5 1/K

ISO 11359-2 | 23°C to 150°C

Coefficient of thermal expansion, transverse

23.0 °C

6E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion, transverse of 6E-5 1/K

ISO 11359-2 | 23°C to 150°C

Heat deflection temperature, 0.45 MPa

205 °C

Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 205 °C

ISO 75/Be | Edgew 120*10*4 sp=100mm

Heat deflection temperature, 1.80 MPa

200 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 200 °C

ISO 75/Ae | Edgew 120*10*4 sp=100mm

Relative temperature index, electrical

105 °C

Show Supplier Material materials with Relative temperature index, electrical of 105 °C

UL 746B

Relative temperature index, mechanical impact

105 °C

Show Supplier Material materials with Relative temperature index, mechanical impact of 105 °C

UL 746B

Relative temperature index, mechanical strength

105 °C

Show Supplier Material materials with Relative temperature index, mechanical strength of 105 °C

UL 746B

Thermal conductivity

23.0 °C

0.3 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 0.3 W/(m·K)

ISO 8302

Flammability

UL Recognized, 94V-0 Flame Class Rating: ≥1.5mm UL 94 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=101772829- -

Electrical

PropertyTemperatureValueComment

Hot-Wire Ignition

23.0 °C

3 mm

Show Supplier Material materials with Hot-Wire Ignition of 3 mm

≥, UL 746A | PLC 1

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

7.5 g/10min

Show Supplier Material materials with Melt mass-flow rate of 7.5 g/10min

ASTM D 1238 | 337°C/6.6 kgf

Shrinkage

23.0 °C

0.2 %

Show Supplier Material materials with Shrinkage of 0.2 %

SABIC method | on tensile bar

Technological properties

Property
Application areas

Small Appliance, Forward Lighting

Availability

Europe

Features

High Heat Resistance

Processing methods

Middle - Zone 2 Temperature: 360 to 410.0°C
Drying Time: 4 to 6.0hrs
Front - Zone 3 Temperature: 370 to 420.0°C
Drying Temperature: 150°C
Hopper Temperature: 80 to 120.0°C
Nozzle Temperature: 360 to 410.0°C
Rear - Zone 1 Temperature: 350 to 400.0°C
Mold Temperature: 140 to 180.0°C
Melt Temperature: 370 to 410.0°C
Maximum Moisture Content: 0.02%

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.