Description

FLEX NORYL™ WCD933 resin is a flexible, non-reinforced extrudable blend of Polyphenylene Ether (PPE) + Thermoplastic Elastomer (TPE). This material contains non-halogenated flame retardant and performance capable of meeting EN 50265-2-1 requirement. FLEX NORYL WCD795 resin is intended for evaluation in AC cable insulation applications such as HD 21.14 flexible cables. It has a Shore A Hardness reading of 93 and exhibits superior thermal stability, very low water absorption, good electric properties, and low specific gravity. Processing is typically conducted on standard extrusion equipment, and UL 1581 testing is conducted on 2.0mm wire with 0.12mm X 20 stranded copper conductor.

This material data has been provided by Sabic.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyTemperatureValueComment

Limiting oxygen index

23.0 °C

29 %

Show Supplier Material materials with Limiting oxygen index of 29 %

Relative density

23.0 °C

1.33 [-]

Show Supplier Material materials with Relative density of 1.33 [-]

ASTM D 792 |

Mechanical

PropertyTemperatureValueComment

Elongation

23.0 °C

175 %

Show Supplier Material materials with Elongation of 175 %

ISO 527 | break, 50 mm/min

Flexural modulus

23.0 °C

0.1 GPa

Show Supplier Material materials with Flexural modulus of 0.1 GPa

ISO 178 | 12.5 mm/min

Hardness, Shore A

23.0 °C

93 [-]

Show Supplier Material materials with Hardness, Shore A of 93 [-]

ASTM D 2240 | 30S reading

Tensile strength

23.0 °C

9 MPa

Show Supplier Material materials with Tensile strength of 9 MPa

ISO 527 | break, 50 mm/min

Thermal

PropertyValueComment

Brittleness temperature

-40 °C

Show Supplier Material materials with Brittleness temperature of -40 °C

<, ASTM D 746

Glow Wire Ignition Temperature

775 °C

Show Supplier Material materials with Glow Wire Ignition Temperature of 775 °C

IEC 60695-2-13 | 3.0 mm

Flammability

Smoke Density on 0.5mm plaque, Flame, Ds, max: 56- ASTM E 662 <br> Glow Wire Flammability Index 750°C, passes at: 3mm IEC 60695-2-12 <br> Smoke Density on 0.5mm plaque, Non-flame, Ds, max: 152- ASTM E 662

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

600 V

Show Supplier Material materials with Comparative tracking index of 600 V

IEC 60112 |

Dielectric constant, 1MHz

23.0 °C

3 [-]

Show Supplier Material materials with Dielectric constant, 1MHz of 3 [-]

ASTM D 150

Dielectric strength

23.0 °C

22.9 kV/mm

Show Supplier Material materials with Dielectric strength of 22.9 kV/mm

IEC 60243-1 | in oil, 2.0mm

Dissipation factor, 1MHz

23.0 °C

1E-3 [-]

Show Supplier Material materials with Dissipation factor, 1MHz of 1E-3 [-]

ASTM D 150 |

Volume resistivity

23.0 °C

2.00E+15 Ω·cm

Show Supplier Material materials with Volume resistivity of 2.00E+15 Ω·cm

ASTM D 257

Rheological Properties

PropertyValueComment

Melt mass-flow rate

8.5 g/10min

Show Supplier Material materials with Melt mass-flow rate of 8.5 g/10min

ASTM D 1238 | 250°C/10.0 kgf

Technological properties

Property
Application areas

Energy Management, Heavy Vehicles, Wiring Devices, Wire & cable

Availability

Europe,Asia,Americas

Processing methods

Melt Temperature: 220 to 250.0°C
Screen Pack: 150 to 100.0-
Conductor Pre-heat Temperature: 25 to 120.0°C
Cross-head Temperature: 220 to 250.0°C
Feed Zone Temperature: 180 to 220.0°C
Water Bath Temperature: 15 to 60.0°C
Drying Time: 5 to 7.0hrs
Cooling Water Air Gap: 100 to 200.0mm
Head Zone Temperature: 220 to 250.0°C
Middle Zone Temperatures: 220 to 250.0°C
Drying Time (Cumulative): 12hrs
Screw Speed: 15 to 85.0rpm
Neck Temperature: 220 to 250.0°C
Drying Temperature: 75 to 85.0°C
Maximum Moisture Content: 0.02%
Die Temperature: 220 to 250.0°C
Extruder Length/Diameter Ratio (L/D): 22:1 to 26:1-

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.