Description

19 MFR LEXAN High Flow Ductile Copolymerwith 400 nm cut off, available in transparent colors only

This material data has been provided by Sabic.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.2 g/cm³

Show Supplier Material materials with Density of 1.2 g/cm³

ISO 1183

Moisture absorption

23.0 °C

0.15 %

Show Supplier Material materials with Moisture absorption of 0.15 %

ISO 62 | (23°C / 50% RH)

Relative density

23.0 °C

1.2 [-]

Show Supplier Material materials with Relative density of 1.2 [-]

ASTM D 792 |

Water absorption

23.0 °C

0.3 %

Show Supplier Material materials with Water absorption of 0.3 %

ISO 62-1 | (23°C/saturated)

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

2.15 GPa

Show Supplier Material materials with Elastic modulus of 2.15 GPa

ISO 527 | 1 mm/min

Elongation

23.0 °C

120 %

Show Supplier Material materials with Elongation of 120 %

ISO 527 | break, 50 mm/min

Flexural modulus

23.0 °C

2.12 GPa

Show Supplier Material materials with Flexural modulus of 2.12 GPa

ISO 178 | 2 mm/min

Flexural strength

23.0 °C

90 MPa

Show Supplier Material materials with Flexural strength of 90 MPa

ISO 178 | yield, 2 mm/min

Hardness, Rockwell R

23.0 °C

120 [-]

Show Supplier Material materials with Hardness, Rockwell R of 120 [-]

ASTM D 785

Impact strength, Izod notched

23.0 °C

65 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 65 kJ/m²

ISO 180/1A | 80*10*3, 23°C

Impact strength, Izod notched, ASTM

23.0 °C

730 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 730 J/m

ASTM D 256 | notched, 23°C

Tensile strength

23.0 °C

59 MPa

Show Supplier Material materials with Tensile strength of 59 MPa

ISO 527 | break, 50 mm/min

Impact strength, Charpy unnotched

ISO 179/1eU | Unnotch Edgew 80*10*3 sp=62mm, -30°C

Impact strength, Izod unnotched

ISO 180/1U | 80*10*3, -30°C

Thermal

PropertyValueComment

Ball Pressure Test

PASS

IEC 60695-10-2 | 125°C +/- 2°C

Heat deflection temperature, 0.45 MPa

123 °C

Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 123 °C

ASTM D 648 | 3.2 mm, unannealed

Heat deflection temperature, 1.80 MPa

111 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 111 °C

ASTM D 648 | 3.2mm, unannealed

Vicat softening temperature

136 °C

Show Supplier Material materials with Vicat softening temperature of 136 °C

ISO 306 | Rate B/120

Optical

PropertyValueComment

Haze

1 %

Show Supplier Material materials with Haze of 1 %

<, ASTM D 1003 | 2.54 mm

Refractive index

1.58 [-]

Show Supplier Material materials with Refractive index of 1.58 [-]

ASTM D542

Transmission

88 %

Show Supplier Material materials with Transmission of 88 %

ASTM D 1003 | 2.54 mm

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

19 g/10min

Show Supplier Material materials with Melt mass-flow rate of 19 g/10min

ASTM D 1238 | 300°C/1.2 kgf

Melt volume-flow rate

16 cm³/10min

Show Supplier Material materials with Melt volume-flow rate of 16 cm³/10min

ISO 1133 | MVR at 300°C/1.2 kg

Shrinkage

23.0 °C

0.5 %

Show Supplier Material materials with Shrinkage of 0.5 %

SABIC method | 3.2 mm

Technological properties

Property
Application areas

Safety Glasses, Individual Equiptment, Exercise Equipment

Availability

Europe,Asia,Americas

Features

High Flow

Processing methods

Vent Depth: 0.038 to 0.076mm
Rear - Zone 1 Temperature: 240 to 280.0°C
Drying Time (Cumulative): 24hrs
Mold Temperature: 50 to 80.0°C
Shot to Cylinder Size: 40 to 60.0%
Nozzle Temperature: 255 to 300.0°C
Middle - Zone 2 Temperature: 250 to 295.0°C
Drying Time: 3 to 4.0hrs
Front - Zone 3 Temperature: 260 to 305.0°C
Back Pressure: 0.3 to 0.7MPa
Screw Speed: 35 to 75.0rpm
Drying Temperature: 105 to 110.0°C
Melt Temperature: 260 to 305.0°C

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.