LEXAN™ Copolymer CXT19EX - Europe

Want to keep this datasheet? Save it now in your required format

Description

LEXAN™ CXT19EX resin is a High Heat Polycarbonate Copolymer Resin with Vicat of 190°C and crystal clear transparency. This resin is optimized for sheet and film extrusion applications, has a low plateout and a broad processing window with limited yellowing. It is available in limited transparent colors.

This material data has been provided by Sabic.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.22 g/cm³

Show Supplier Material materials with Density of 1.22 g/cm³

ISO 1183

Moisture absorption

23.0 °C

0.3 %

Show Supplier Material materials with Moisture absorption of 0.3 %

ISO 62 | (23°C / 50% RH)

Relative density

23.0 °C

1.22 [-]

Show Supplier Material materials with Relative density of 1.22 [-]

ASTM D 792 |

Water absorption

23.0 °C

0.5 %

Show Supplier Material materials with Water absorption of 0.5 %

ISO 62-1 | (23°C/saturated)

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

2.5 GPa

Show Supplier Material materials with Elastic modulus of 2.5 GPa

ISO 527 | 1 mm/min

Elongation

23.0 °C

7.5 %

Show Supplier Material materials with Elongation of 7.5 %

ISO 527 | yield, 50 mm/min

Flexural modulus

23.0 °C

2.55 GPa

Show Supplier Material materials with Flexural modulus of 2.55 GPa

ISO 178 | 2 mm/min

Flexural strength

23.0 °C

120 MPa

Show Supplier Material materials with Flexural strength of 120 MPa

ISO 178 | yield, 2 mm/min

Impact strength, Charpy notched

23.0 °C

9 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 9 kJ/m²

ISO 179/1eA | V-notch Edgew 80*10*3 sp=62mm, 23°C

Impact strength, Izod notched

23.0 °C

6 kJ/m²

Show Supplier Material materials with Impact strength, Izod notched of 6 kJ/m²

ISO 180/1A | notched 80*10*3, -30°C

Impact strength, Izod notched, ASTM

23.0 °C

70 J/m

Show Supplier Material materials with Impact strength, Izod notched, ASTM of 70 J/m

ASTM D 256 | notched, -30°C

Tensile strength

23.0 °C

80 MPa

Show Supplier Material materials with Tensile strength of 80 MPa

ISO 527 | yield, 50 mm/min

Impact strength, Charpy unnotched

ISO 179/1eU | Unnotch Edgew 80*10*3 sp=62mm, 23°C

Impact strength, Izod unnotched

ISO 180/1U | unnotched 80*10*3, 23°C,

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

6E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 6E-5 1/K

ISO 11359-2 | -40°C to 40°C

Coefficient of thermal expansion, transverse

23.0 °C

6E-5 1/K

Show Supplier Material materials with Coefficient of thermal expansion, transverse of 6E-5 1/K

ISO 11359-2 | -40°C to 40°C

Glass transition temperature

195 °C

Show Supplier Material materials with Glass transition temperature of 195 °C

SABIC method | (half width)

Heat deflection temperature

172 - 187 °C

Show Supplier Material materials with Heat deflection temperature of 172 - 187 °C

Heat deflection temperature, 0.45 MPa

187 °C

Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 187 °C

ISO 75/Bf | Flatw 80*10*4 sp=64mm

Heat deflection temperature, 1.80 MPa

172 °C

Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 172 °C

ISO 75/Af | Flatw 80*10*4 sp=64mm

Thermal conductivity

23.0 °C

0.2 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 0.2 W/(m·K)

ISO 8302

Vicat softening temperature

192 °C

Show Supplier Material materials with Vicat softening temperature of 192 °C

ISO 306 | Rate B/120

Optical

PropertyValueComment

Refractive index

1.61 [-]

Show Supplier Material materials with Refractive index of 1.61 [-]

ISO 489

Transmission

87 %

Show Supplier Material materials with Transmission of 87 %

ASTM D1003 | at 3.0 mm

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

15 g/10min

Show Supplier Material materials with Melt mass-flow rate of 15 g/10min

ASTM D 1238 | 330°C/2.16 kgf

Melt volume-flow rate

13 cm³/10min

Show Supplier Material materials with Melt volume-flow rate of 13 cm³/10min

ISO 1133 | MVR at 330°C/2.16kg

Shrinkage

23.0 °C

0.7 %

Show Supplier Material materials with Shrinkage of 0.7 %

SABIC method | 3.2 mm

Shrinkage, transverse

23.0 °C

0.7 %

Show Supplier Material materials with Shrinkage, transverse of 0.7 %

SABIC method | 3.2 mm

Technological properties

Property
Application areas

Personal safety, High heat films, Sensor lens, Flash lens, Camera lens, Displays, Electronic Components, Forward Lighting

Availability

Europe,Asia,Americas

Features

High Heat Resistance

Processing methods

Barrel - Zone 1 Temperature: 180 to 250.0°C
Barrel - Zone 2 Temperature: 270 to 310.0°C
Barrel - Zone 3 Temperature: 300 to 350.0°C
Hopper Temperature: 100 to 150.0°C
Adapter Temperature: 290 to 340.0°C
Die Temperature: 290 to 355.0°C
Melt Temperature: 290 to 355.0°C
Calibrator Temperature: 100 to 170.0°C
Drying Temperature: 135°C
Drying Time: 4 to 6.0hrs

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.